Carbon-coated ferric pyrophosphate precursor material as well as preparation method and application thereof
The carbon-coated ferric pyrophosphate precursor material is prepared by the spray drying-calcination method, which solves the problems of difficult material morphology control and long process cycle in the existing technology, and realizes the preparation of high-efficiency and low-cost cathode materials for sodium ion batteries. , improving the stability and conductivity of the material.
Patent Information
- Application Number
- CN202410855091.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-28
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2044-06-28
AI Technical Summary
The existing preparation process of sodium-ion battery cathode materials has problems such as difficulty in controlling material morphology, uneven carbon coating, long process cycle, high cost and low stability, especially the sanding+spraying method and the sol-gel method. There are defects in material shrinkage and deformation.
The carbon-coated ferric pyrophosphate precursor material is prepared using a spray drying-calcination method. The phosphorus source, carbon source, and iron source are dissolved in a medium solution to form a slurry. After spray drying, it is calcined in an inert protective gas to obtain a uniform The carbon-coated ferric pyrophosphate precursor material is mixed with a sodium source and calcined to obtain a sodium ferric pyrophosphate material.
It has achieved a positive electrode material with no agglomeration and good conductivity, simplified the preparation process, reduced the cost, improved the controllability and stability of the material, and the process is simple and suitable for market production.
Smart Images

Figure CN118851144A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of sodium ion battery positive electrode materials and relates to a positive electrode material precursor, in particular to a carbon-coated phosphate iron pyrophosphate precursor material and a preparation method and application thereof. Background Art
[0002] Positive electrode materials for sodium ion batteries include transition metal oxides, Prussian blue analogues, polyanion compounds, etc. Among them, the polyanion compound with NASICON structure is a three-dimensional framework structure composed of strong covalent bonds. It not only has high structural stability, but also has a fast sodium ion diffusion rate, and the volume change and phase change are small during ion insertion and extraction, making it widely used in the preparation of positive electrode materials for sodium ion batteries.
[0003] CN117361482A discloses a preparation method and application of a composite phosphate pyrophosphate polyanion positive electrode material. The sodium iron phosphate pyrophosphate positive electrode material is prepared by sand milling + spraying. The sodium source, phosphorus source and iron source are directly mixed by sand milling, which has problems such as difficulty in controlling the material morphology and uneven carbon coating.
[0004] CN116924371A discloses a method for preparing a core-shell structured sodium iron manganese phosphate pyrophosphate cathode material, wherein the sodium iron manganese phosphate pyrophosphate cathode material is prepared by a sol-gel method. The raw materials of the sol-gel method are expensive, and some of the raw materials are organic matter. The gas and organic matter released during drying are harmful to the human body, and the material shrinks and deforms greatly. In addition, the sol-gel process has a long preparation cycle, which is not conducive to marketization. Summary of the invention
[0005] In view of the above problems existing in the prior art, in the first aspect, the present invention provides a carbon-coated iron phosphate pyrophosphate precursor material and a preparation method thereof; in the second aspect, the present invention provides a sodium iron phosphate pyrophosphate and a preparation method thereof.
[0006] First, the present invention provides a method for preparing a carbon-coated iron phosphate pyrophosphate precursor material, comprising the following steps: Step 1, dissolving a phosphorus source, a carbon source, and an iron source in a medium solution to obtain slurry A; Step 2, spray drying slurry A to obtain mixed powder B; Step 3, calcining the mixed powder B in an inert protective gas, cooling, crushing and sieving the calcined product to obtain a carbon-coated iron phosphate pyrophosphate precursor material.
[0007] Preferably, the molar ratio of P:Fe in the phosphorus source and the iron source is 9-13:8-10.
[0008] Preferably, the phosphorus source is one or more of ammonium dihydrogen phosphate, diammonium hydrogen phosphate, aminotrimethylenephosphonic acid, ethylenediaminetetramethylenephosphonic acid, hexamethylenediaminetetramethylenephosphonic acid, hydroxyethylidene diphosphonic acid, ferric phosphate, ferrous phosphate, ferric pyrophosphate, ferrous pyrophosphate, ferric hypophosphite, and glyceroferric phosphate; More preferably, the carbon source is one or more of citric acid, oxalic acid, CNTs, oleic acid, graphene, pyromellitic acid, glucose, ethylene glycol, polyethylene glycol, liquid paraffin, PVP, bituminous coal, phenolic resin, soft carbon, MCMB, polyacrylonitrile, stearic acid, ascorbic acid, PPy, Super P, polyaniline, soluble starch, cellulose, and sucrose; More preferably, the iron source is one or more of ferrous oxalate, ferric nitrate, iron powder, ferric phosphate, ferrous citrate, ferrous acetate, ferrous formate, ferric pyrophosphate, ferrous pyrophosphate, ferrous phosphate, ferrous oxide, and ferrous oxide. More preferably, the medium solution includes one or more of water, anhydrous ethanol, and ethylene glycol solution.
[0009] Preferably, in step 1, when dissolving the phosphorus source, carbon source and iron source, the stirring rate is 100-1600 rpm and the stirring time is 2-10 h.
[0010] Preferably, in step 1, the solid content of the slurry A is 30% to 70%.
[0011] Preferably, in step 2, the inlet air temperature of the spray drying is 200-300°C; the outlet air temperature of the spray drying is 90-150°C; the fan frequency is 30-50 Hz; and the peristaltic speed is 60-150 rpm.
[0012] Preferably, in step 3, the calcination temperature is 350-900° C. and the calcination time is 4-20 hours.
[0013] Preferably, the inert protective gas is one or both of argon and nitrogen.
[0014] Preferably, in step 3, the comminution process is any one of grinding, air flow crushing and vibration crushing.
[0015] Preferably, in step 3, when sieving, the mesh size of the sieve is 50-500 mesh.
[0016] In a second aspect, based on the same inventive concept, the present invention provides ferric phosphate pyrophosphate, which is prepared by the above preparation method.
[0017] Preferably, the carbon content of the ferric phosphate pyrophosphate precursor material is 0.2% to 12%.
[0018] Preferably, the particle size D50 of ferric phosphate pyrophosphate is 3.24-4.75 μm; the specific surface area is 12-16 m 2 / g; tap density is 1.4~1.7g / cm 3 .
[0019] In a third aspect, based on the same inventive concept, the present invention provides a sodium iron phosphate pyrophosphate material, which is obtained by mixing the above-mentioned carbon-coated sodium iron phosphate pyrophosphate precursor material and a sodium source, and calcining the mixture under an inert protective gas.
[0020] Preferably, the sodium source is one or more of sodium carbonate, sodium hydroxide, sodium pyrophosphate, sodium bicarbonate, sodium dihydrogen phosphate, disodium hydrogen phosphate, and sodium phosphate.
[0021] Preferably, the mass ratio of the ferric phosphate pyrophosphate precursor material to the sodium source is 1:0.14-0.98.
[0022] Preferably, the calcination temperature is 350-1000° C., and the calcination time is 4-12 hours.
[0023] More preferably, during calcination, the heating rate is 1-10°C / min; and the cooling rate is 1-10°C / min.
[0024] Preferably, the inert protective gas is one or both of argon and nitrogen.
[0025] In a fourth aspect, based on the same negative concept, the present invention provides a sodium ion battery, wherein the positive electrode material is prepared by the preparation method of the above-mentioned carbon-coated sodium iron phosphate pyrophosphate material.
[0026] The above technical solution provided by the present invention has at least one or more of the following obvious beneficial technical effects: (1) The present invention prepares carbon-coated iron phosphate pyrophosphate Fe by spray drying-calcination method x (PO 4 ) y (P 2 O 7 ) z @C precursor material, the obtained precursor material has no agglomeration phenomenon and is evenly coated with carbon. x (PO 4 ) y (P 2 O 7 ) z @C The positive electrode material made from precursor material has good conductivity and simple preparation process, which is conducive to marketization.
[0027] (2) by mixing the phosphate pyrophosphate iron Fe prepared by the present invention x (PO4 ) y (P 2 O 7 ) z @C precursor material and sodium source are calcined to obtain sodium iron phosphate pyrophosphate material. The prepared sodium iron phosphate pyrophosphate material has uniform particle size distribution and no agglomeration.
[0028] (3) By adjusting the iron phosphate pyrophosphate Fe x (PO 4 ) y (P 2 O 7 ) z @C The size, specific surface area, tap density, carbon content and other parameters of the precursor material are used to adjust the relevant parameters of the final sodium iron pyrophosphate material.
[0029] (4) Compared with the prior art of preparing sodium iron pyrophosphate materials by sand milling + spraying process or sol-gel process, the synthesis preparation process of the NFPP sodium electrode precursor proposed in the present invention is short, low in synthesis difficulty, low in cost, high in controllability, and the obtained positive electrode material has high stability. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] Figure 1 This is the XRD pattern of the carbon-coated iron phosphate pyrophosphate precursor material prepared in Example 2 of the present invention.
[0031] Figure 2 This is a SEM image of the carbon-coated iron phosphate pyrophosphate precursor material prepared in Example 1 of the present invention.
[0032] Figure 3 This is an SEM image of the carbon-coated sodium iron pyrophosphate material prepared in Example 5 of the present invention.
[0033] Figure 4 This is a SEM image of the carbon-coated iron phosphate pyrophosphate precursor material prepared in Comparative Example 1 of the present invention.
[0034] Figure 5 Schematic diagram of battery cycle performance of a battery made using the carbon-coated sodium iron phosphate pyrophosphate material prepared in Example 6 of the present invention.
[0035] Figure 6 This is a charge and discharge curve diagram of the carbon-coated sodium iron pyrophosphate material prepared using Example 5 of the present invention. DETAILED DESCRIPTION
[0036] The present invention provides the following specific technical solutions.
[0037] First, the present invention provides a method for preparing a carbon-coated iron phosphate pyrophosphate precursor material, comprising the following steps: Step 1, dissolving a phosphorus source, a carbon source, and an iron source in water, and mixing them evenly to obtain slurry A; Step 2, spray drying slurry A to obtain mixed powder B; Step 3: calcining, cooling, crushing and sieving the mixed powder B in an inert protective gas to obtain a carbon-coated iron phosphate pyrophosphate precursor material.
[0038] Preferably, the molar ratio of P:Fe in the phosphorus source and the iron source is 9-13:8-10.
[0039] In actual situations, the amount of phosphorus source, carbon source and iron source added can be selected according to actual needs, and the molar ratio of P:Fe in phosphorus source and iron source is 9~13:8~10, which is only the preferred range proposed by the inventor. The inventor proposed that different carbon sources have different residual carbon rates at different sintering temperatures, so when mixing the ingredients, the amount of carbon source used can be calculated according to the theoretical carbon content required by the material, the calcination temperature and the thermogravimetric weight of the carbon source.
[0040] Preferably, the phosphorus source is one or more of ammonium dihydrogen phosphate, diammonium hydrogen phosphate, aminotrimethylenephosphonic acid, ethylenediaminetetramethylenephosphonic acid, hexamethylenediaminetetramethylenephosphonic acid, hydroxyethylidene diphosphonic acid, ferric phosphate, ferrous phosphate, ferric pyrophosphate, ferrous pyrophosphate, ferric hypophosphite, and glyceroferric phosphate.
[0041] Preferably, the carbon source is one or more of citric acid, oxalic acid, CNTs, oleic acid, graphene, pyromellitic acid, glucose, ethylene glycol, polyethylene glycol, liquid paraffin, PVP, bituminous coal, phenolic resin, soft carbon, MCMB, polyacrylonitrile, stearic acid, ascorbic acid, PPy, Super P, polyaniline, soluble starch, cellulose, and sucrose.
[0042] Preferably, the iron source is one or more of ferrous oxalate, ferric nitrate, iron powder, ferric phosphate, ferrous citrate, ferrous acetate, ferrous formate, ferric pyrophosphate, ferrous pyrophosphate, ferrous phosphate, ferrous oxide, and ferrous oxide; and the medium solution includes one or more of water, anhydrous ethanol, and ethylene glycol solution.
[0043] Preferably, in step 1, when dissolving the phosphorus source, carbon source and iron source, the stirring rate is 100-1600 rpm and the stirring time is 2-10 h.
[0044] In actual situations, the stirring rate and stirring time can be selected according to actual needs, as long as the phosphorus source, carbon source and iron source are completely dissolved.
[0045] Preferably, the solid content of the slurry A is 30% to 70%.
[0046] The inventors have found through research that if the solid content in slurry A is too high, it is not conducive to the dispersion of materials in the subsequent spray drying process; if the solid content is too low, it will increase the time consumption of spray drying, increase the energy consumption, and increase the cost. In practical applications, the solid content in slurry A can be selected according to actual needs. In a specific embodiment of the present invention, the solid content in slurry A can be 30%, 40%, 50%, 60%, or 70%.
[0047] Preferably, in step 2, the inlet air temperature of the spray drying is 200-300°C; the outlet air temperature of the spray drying is 90-150°C; the fan frequency is 30-50 Hz; and the peristaltic speed is 60-150 rpm.
[0048] In practical applications, the inlet temperature, outlet temperature, fan frequency and peristaltic speed during spray drying can be adjusted according to actual conditions. In a specific embodiment of the present invention, the inlet temperature can be 200°C, 210°C, 220°C, 230°C, 240°C, 250°C, or 300°C; the outlet temperature can be 90°C, 100°C, 110°C, 120°C, 130°C, 140°C, or 150°C; the fan frequency can be 30Hz, 35Hz, 40Hz, 45Hz, or 50Hz; and the peristaltic speed can be 60rpm, 80rpm, 100rpm, 120rpm, or 150rpm.
[0049] Preferably, in step 3, the calcination temperature is 350-900° C., and the calcination time is 4-20 hours.
[0050] In practical applications, the calcination temperature and calcination time can be adjusted according to actual needs. In a specific embodiment of the present invention, the calcination temperature can be 350°C, 400°C, 500°C, 600°C, 700°C, 850°C, or 900°C; the calcination time can be 4h, 6h, 8h, 10h, 12h, 15h, 17h, or 20h.
[0051] More preferably, in step 3, during calcination, the heating rate is 1-10°C / min; and the cooling rate is 1-10°C / min.
[0052] In practical applications, the heating rate and cooling rate during calcination can be selected according to actual needs. In a specific embodiment of the present invention, the heating rate can be 1°C / min, 3°C / min, 5°C / min, 8°C / min, and 10°C / min; the cooling rate can be 1°C / min, 3°C / min, 5°C / min, 7°C / min, 8°C / min, and 10°C / min.
[0053] Preferably, the inert protective gas is one or both of argon and nitrogen.
[0054] Preferably, in step 3, the comminution process is any one of grinding, air flow crushing and vibration crushing.
[0055] Preferably, in step 3, when sieving, the mesh size of the sieve is 50-500 mesh.
[0056] In a second aspect, based on the same inventive concept, the present invention provides ferric phosphate pyrophosphate, which is prepared by the above preparation method.
[0057] In the third aspect, based on the same inventive concept, the present invention provides a method for preparing sodium ferric pyrophosphate, comprising the following steps: The above-mentioned phosphate iron pyrophosphate and sodium source are mixed, calcined in an inert protective gas, and cooled to obtain the phosphate iron pyrophosphate sodium material.
[0058] In the prior art, the phosphorus source, carbon source, iron source and sodium source are usually directly mixed and calcined under a protective gas to prepare the sodium ferric phosphate pyrophosphate material, and the particles are easy to agglomerate and the morphology is uncertain. The inventors have found that the phosphate pyrophosphate iron precursor is first prepared, and then the sodium source is mixed and calcined under an inert protective gas. The obtained sodium ferric phosphate pyrophosphate material particles are spherical, without agglomeration, and evenly distributed. And by regulating the morphology of the phosphate pyrophosphate iron precursor, the morphology of the sodium ferric phosphate pyrophosphate material can be controlled to a certain extent, reducing the difficulty of synthesis and improving controllability.
[0059] Preferably, the sodium source is one or more of sodium carbonate, sodium hydroxide, sodium pyrophosphate, sodium bicarbonate, sodium dihydrogen phosphate, disodium hydrogen phosphate, sodium phosphate, sodium acetate, and sodium oxalate.
[0060] Preferably, the mass ratio of the ferric phosphate pyrophosphate precursor material to the sodium source is 1:0.14-0.98.
[0061] In actual situations, the sodium source can be selected according to actual needs. The inventors have found through research that too much sodium source will easily lead to an increase in residual alkali in the subsequent synthesis process of sodium ferric phosphate pyrophosphate, while too little sodium source will lead to a low gram capacity of the material.
[0062] Preferably, the calcination temperature is 350-1000° C., and the calcination time is 4-12 hours.
[0063] In a specific embodiment of the present invention, the calcination temperature can be 350°C, 400°C, 500°C, 550°C, 600°C, or 700°C; and the calcination time can be 4h, 6h, 8h, 10h, or 12h.
[0064] More preferably, during calcination, the heating rate is 1-10°C / min; and the cooling rate is 1-10°C / min.
[0065] In actual situations, the heating rate and cooling rate can be selected according to actual needs. In a specific embodiment of the present invention, the heating rate can be 1°C / min, 3°C / min, 5°C / min, 8°C / min, and 10°C / min; the cooling rate can be 1°C / min, 3°C / min, 5°C / min, 8°C / min, and 10°C / min. In other cases, the material can also be taken out and cooled naturally.
[0066] Preferably, the inert protective gas is one or both of argon and nitrogen.
[0067] In order to make the technical problems to be solved, technical solutions and technical advantages of the present invention more clear, they will be described in detail below with reference to specific examples, but the protection scope of the present invention is not limited to the following specific embodiments.
[0068] Unless otherwise defined, all professional terms used below have the same meanings as those generally understood by those skilled in the art. The professional terms used herein are only for the purpose of describing specific embodiments and are not intended to limit the scope of protection of the present invention.
[0069] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in the present invention can be purchased from the market or prepared by existing methods.
[0070] Embodiment 1: A method for preparing a carbon-coated iron phosphate pyrophosphate precursor material comprises the following steps: Step 1, mix 3 mol of ferric phosphate, 1.5 mol of ferric pyrophosphate, and 0.75 mol of citric acid, add into water, set the sand mill speed to 800 rpm, sand mill for 6 hours, and obtain slurry A, the solid content in slurry A is 50%.
[0071] Step 2, spray drying slurry A, the feed creeping speed is 100 rpm, the air inlet temperature is 240°C, the air outlet temperature is 120°C, and the fan frequency is 45 Hz to obtain mixed powder B; Step 3, calcining the mixed powder B in a nitrogen atmosphere with an internal oxygen value of 50 ppm. The temperature was raised to 700°C at a heating rate of 5°C / min, kept at 700°C for 10 hours, cooled to room temperature at a cooling rate of 7°C / min, and then taken out, crushed by air flow, and sieved with a 300-mesh sieve to obtain a carbon-coated iron phosphate pyrophosphate precursor material with a particle size of 3.66 μm.
[0072] Embodiment 2: Step 1, mix 4 mol of glyceroferric phosphate, 2 mol of ferrous pyrophosphate, and 0.5 mol of glucose, add into water, stir at a stirring rate of 100 rpm for 2 hours, and prepare slurry A, the solid content in slurry A is 30%.
[0073] Step 2, spray drying slurry A, the feed creeping speed is 60 rpm, the air inlet temperature is 200°C, the air outlet temperature is 90°C, and the fan frequency is 30 Hz to obtain mixed powder B; Step 3, calcining the mixed powder B in an argon atmosphere with an internal oxygen value of 10 ppm. The temperature was raised to 350°C at a rate of 1°C / min, kept at that temperature for 4 hours, and then cooled to room temperature at a rate of 1°C / min, taken out, and crushed by vibration, and sieved with a 50-mesh sieve to obtain a carbon-coated iron phosphate pyrophosphate precursor material with a particle size of 3.51 μm.
[0074] Embodiment 3: Step 1, mix 12 mol of ammonium dihydrogen phosphate, 9 mol of ferrous citrate, and 0.5 mol of sucrose, add into water, and stir for 10 hours at a sand milling rate of 1600 rpm to obtain slurry A, wherein the solid content of slurry A is 70%.
[0075] Step 2, spray drying slurry A, the feed creeping speed is 150 rpm, the air inlet temperature is 300°C, the air outlet temperature is 150°C, and the fan frequency is 50 Hz to obtain mixed powder B; Step 3, calcining the mixed powder B in a nitrogen atmosphere with an internal oxygen value of 100 ppm. The temperature was raised to 900°C at a rate of 10°C / min, kept at that temperature for 20 hours, cooled to room temperature at a rate of 10°C / min, taken out, ground, and sieved with a 500-mesh sieve to obtain a carbon-coated iron phosphate pyrophosphate precursor material with a particle size of 4.42 μm.
[0076] Embodiment 4: Step 1, mix 9 mol of ferric phosphate hydrate and 0.1 mol of ascorbic acid, add into water, sand grind at a speed of 1600 rpm, sand grind for 3.5 hours and stir evenly to obtain slurry A.
[0077] Step 2, spray drying slurry A, the feed creeping speed is 125 rpm, the air inlet temperature is 250°C, the air outlet temperature is 130°C, and the fan frequency is 50 Hz to obtain mixed powder B; Step 3, calcining the mixed powder B in a nitrogen atmosphere with an oxygen content of 100 ppm. The temperature was raised to 850°C at a heating rate of 8°C / min, maintained for 15 hours, and then cooled to room temperature at a cooling rate of 10°C / min, taken out, ground, and sieved using a 500-mesh sieve to obtain a carbon-coated iron phosphate pyrophosphate precursor material with a particle size of 4.03 μm.
[0078] Embodiment 5: A method for preparing sodium ferric pyrophosphate comprises the following steps: 5 kg of the carbon-coated phosphate iron pyrophosphate material prepared in Example 1 and 3.09 kg of sodium acetate were mixed, the mixing speed was controlled to 900 rpm, the mixing time was 30 min, and the mixture was calcined at 550° C. for 10 h under a nitrogen atmosphere to obtain sodium iron pyrophosphate.
[0079] Embodiment 6: A method for preparing sodium ferric pyrophosphate comprises the following steps: Mix 6 kg of carbon-coated ferric phosphate pyrophosphate material prepared in Example 2 with 3.8 kg of sodium carbonate and 1.5 kg of sodium phosphate, control the mixing speed to 150 rpm, the mixing time to 15 min, and calcine at 950° C. for 4 h under a nitrogen atmosphere to obtain sodium ferric pyrophosphate.
[0080] Embodiment 7: A method for preparing sodium ferric pyrophosphate comprises the following steps: 4 kg of the carbon-coated ferric pyrophosphate material prepared in Example 3 and 2.17 kg of sodium oxalate were mixed, the mixing speed was controlled to 1000 rpm, the mixing time was 40 min, and the mixture was calcined at 900° C. for 12 h under a nitrogen atmosphere to obtain sodium ferric pyrophosphate.
[0081] Embodiment 8: Mix 3 kg of carbon-coated ferric phosphate pyrophosphate material prepared in Example 4 with 0.5 kg of sodium bicarbonate and 0.65 kg of sodium phosphate, control the mixing speed to 150 rpm, the mixing time to 15 min, and calcine at 850° C. for 4 h under a nitrogen atmosphere to obtain sodium ferric pyrophosphate.
[0082] Comparative Example 1: A method for preparing a carbon-coated iron phosphate pyrophosphate precursor material comprises the following steps: Step 1, mix 3 mol of ferric phosphate, 1.5 mol of ferric pyrophosphate, and 0.75 citric acid, add into water, set the sand mill speed to 800 rpm, sand mill for 6 hours, and obtain slurry A, the solid content of the mixed solution is 50%.
[0083] Step 2: After vacuum drying, slurry A was placed in a nitrogen atmosphere for calcination, and the internal oxygen value was 50 ppm. The temperature was raised to 600°C at a rate of 5°C / min for 120 minutes, and then kept at 600°C for 10 hours. The temperature was lowered to room temperature at a rate of 6°C / min, and then taken out, broken by air flow, and sieved with a 250-mesh screen to obtain a carbon-coated iron phosphate pyrophosphate precursor material with a particle size of 4.99 μm.
[0084] Comparative Example 2: Step 1, mixing 4 mol of glyceroferric phosphate and 2 mol of ferrous pyrophosphate, adding into water, stirring at a rate of 100 rpm for 2 hours, to obtain slurry A, wherein the solid content of slurry A is 30%; Step 2, spray drying slurry A, the feed creeping speed is 90 rpm, the air inlet temperature is 240°C, the air outlet temperature is 105°C, and the fan frequency is 40 Hz to obtain mixed powder B; Step 3, after mixing 0.5 mol of glucose and mixed powder B to obtain mixed powder C, the mixed powder C is placed in an inert protective gas for calcination, and the internal oxygen value is 10 ppm. The temperature is raised to 550°C at a heating rate of 1°C / min, kept warm for 6 hours, cooled to room temperature at a cooling rate of 4°C / min, and then taken out. The calcined product is cooled, air flow crushed, and sieved with a 250-mesh sieve to obtain a carbon-coated iron phosphate pyrophosphate precursor material with a particle size of 4.87 μm.
[0085] Comparative Example 3: Step 1, 12 mol of ammonium dihydrogen phosphate and 9 mol of ferrous citrate were mixed, added into water, and stirred for 10 hours at a sand milling rate of 1600 rpm to obtain slurry A, wherein the solid content of slurry A was 70%; Step 2, spray drying slurry A, the feed creeping speed is 155 rpm, the air inlet temperature is 290°C, the air outlet temperature is 150°C, and the fan frequency is 50 Hz to obtain mixed powder B; Step 3, calcining the mixed powder B under a nitrogen atmosphere, with an internal oxygen value of 100ppm. The temperature was raised to 850°C at a heating rate of 10°C / min, kept at this temperature for 20h, cooled to room temperature at a cooling rate of 10°C / min, and then taken out, and then the calcined product and 0.5mol sucrose were mixed to obtain a mixed powder C. After calcining the mixed powder C again, the temperature was raised to 500°C at a heating rate of 5°C / min, kept at this temperature for 5h, cooled to room temperature at a cooling rate of 6°C / min, and then taken out, cooled, crushed, and sieved to obtain a carbon-coated iron phosphate pyrophosphate precursor material.
[0086] Comparative Example 4: Step 1: Mix ferric phosphate, sodium carbonate, glucose, sodium dihydrogen phosphate, and pure water to control Fe:P:Na=3:4:4, solid content of 60%, carbon content of 2%, and sand grind to obtain slurry A at a sand grinding speed of 200 rpm for 10 hours; Step 2: spray drying the slurry A to obtain powder B, controlling the spray drying air inlet temperature to 220°C, the creeping speed to 160 rpm, and the air outlet temperature to 110°C; Step 3: calcine the mixed powder B in a nitrogen atmosphere with an oxygen content of 100 ppm. The temperature is raised to 550°C at a rate of 5°C / min for 87.5 min, maintained for 12 h, and then cooled to room temperature at a rate of 10°C / min, taken out, ground, and sieved with a 500-mesh sieve to obtain carbon-coated sodium iron phosphate with a particle size of 5.15 μm.
[0087] Comparative Example 5: Step 1: Add 2.15 kg of sodium carbonate, 5.95 kg of ammonium phosphate, 1 kg of glucose and 1 kg of stearic acid into deionized water, control the solid content to 55%, and stir until a transparent solution A is obtained.
[0088] Step 2: Add 4.35 kg of ferrous oxalate, 8.2 kg of ethylenediaminetetraacetic acid, and 0.55 kg of hexadecyltrimethylammonium bromide into 20 l of deionized water and stir magnetically until a transparent solution B is obtained.
[0089] Step 3: Then drop the clear solution B into solution A and stir vigorously. Then heat the mixed solution in a water bath at 90°C until all the excess water is removed to obtain the sol-gel precursor: Step 4: Grind the precursor into fine powder, perform intermediate grinding at 900°C in a high-purity argon atmosphere, and anneal for 24h to finally obtain sodium iron pyrophosphate with a particle size of 5.24μm.
[0090] The conductivity test method of the precursor materials prepared in Examples 1 to 4 and Comparative Examples 1 to 3, and the positive electrode materials prepared in Examples 5 to 8 and Comparative Examples 4 to 5 is as follows: Weigh 1g of sample, calibrate the conductivity meter with calibration liquid, place the sample between the four probes to ensure good contact between the probes, adjust the sample height to 20mm, and when the pressure reaches 8Mpa, calculate the resistance by measuring the current and voltage drop, and calculate the conductivity by the geometric dimensions. The test results are shown in Table 1 below.
[0091] Table 1 - Performance parameters of precursor materials obtained in Examples 1 to 4 and Comparative Examples 1 to 3 It can be seen from Table 1 that the precursor materials prepared in Examples 1 to 4 and Comparative Examples 1 to 3 have a larger tap density and a larger specific surface area.
[0092] Table 2 - Performance parameters of positive electrode materials obtained in Examples 5 to 8 and Comparative Examples 4 to 5 It can be seen from Table 2 that the positive electrode material prepared by the preparation process for preparing the positive electrode material provided by the present invention has a larger tap density and a larger specific surface area. After the precursor provided by the present invention and the sodium source are mixed and reacted, the internal particles become larger, resulting in a thinner carbon thickness coated on the surface of the positive electrode material, which affects the electronic conductivity.
[0093] The sodium iron phosphate pyrophosphate positive electrode materials prepared in Examples 5 to 8 and Comparative Examples 4 to 5 are assembled into button batteries, comprising the following steps: 1) Stirring the mixture for 6 hours using NMP as solvent in a ratio of active material: conductive agent: binder = 9:0.5:0.5; 2) Coat the slurry on 16 μm aluminum foil, control the coating thickness to 150 μm, and bake in a vacuum oven at 105 °C for 4 h; 3) The pole piece is cut into small discs after rolling; 4) Assemble the positive electrode shell-positive electrode sheet-diaphragm-sodium sheet-negative electrode shell, and add 5 drops of sodium electrolyte; 5) After standing for 12 hours, conduct charge and discharge tests at a current density of 100 mA / g at room temperature and a test voltage range of 0.01 to 3.0 V.
[0094] Figure 5 A schematic diagram of battery cycle performance of a battery made using the carbon-coated sodium iron phosphate pyrophosphate material made in Example 6 of the present invention; Figure 6 This is a charge and discharge curve diagram of the carbon-coated sodium iron pyrophosphate material prepared using Example 5 of the present invention.
[0095] Table 2 - Cycle parameters of button cells assembled from sodium iron phosphate pyrophosphate cathode materials obtained in Examples 5 to 8 and Comparative Examples 4 to 5 As can be seen from Table 2, the batteries assembled from the positive electrode materials prepared in Examples 5 to 8 have superior discharge specific capacity and cycle stability compared to the batteries assembled from the positive electrode materials prepared in Comparative Examples 4 to 5.
[0096] Figure 1 This is the XRD pattern of the carbon-coated iron phosphate pyrophosphate precursor material prepared in Example 2 of the present invention.
[0097] Figure 2 This is a SEM image of the carbon-coated ferric phosphate pyrophosphate precursor material prepared in Example 1 of the present invention. It can be seen that the precursor material particles prepared in Example 1 are spherical. Figure 3 This is a SEM image of the carbon-coated sodium iron pyrophosphate material prepared in Example 5 of the present invention, compared with Figure 2 and Figure 3 It can be seen that the morphology of the final cathode material can be adjusted by adjusting the morphology of the precursor.
[0098] Figure 4 This is a SEM image of the carbon-coated iron phosphate pyrophosphate precursor material prepared in Comparative Example 1 of the present invention. Figure 3 and Figure 4 The particle distribution is more uniform, the carbon coating is uniform, and there is no agglomeration.
[0099] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A method for preparing a carbon-coated iron phosphate pyrophosphate precursor material, characterized in that: The following steps are involved: Step 1, dissolving a phosphorus source, a carbon source, and an iron source in a medium solution to obtain slurry A; Step 2, spray drying slurry A to obtain mixed powder B; Step 3, calcining the mixed powder B in an inert protective gas, cooling, crushing and sieving the calcined product to obtain a carbon-coated iron phosphate pyrophosphate precursor material.
2. The method for preparing the carbon-coated phosphate iron pyrophosphate precursor material according to claim 1, characterized in that: The molar ratio of P:Fe in the phosphorus source and the iron source is 9~13:8~10.
3. The method for preparing the carbon-coated phosphate iron pyrophosphate precursor material according to claim 1 or 2, characterized in that: The phosphorus source is one or more of ammonium dihydrogen phosphate, diammonium hydrogen phosphate, aminotrimethylenephosphonic acid, ethylenediaminetetramethylenephosphonic acid, hexamethylenediaminetetramethylenephosphonic acid, hydroxyethylidene diphosphonic acid, ferric phosphate, ferrous phosphate, ferric pyrophosphate, ferrous pyrophosphate, ferric hypophosphite, and glyceroferric phosphate; More preferably, the carbon source is one or more of citric acid, oxalic acid, CNTs, oleic acid, graphene, pyromellitic acid, glucose, ethylene glycol, polyethylene glycol, liquid paraffin, PVP, bituminous coal, phenolic resin, soft carbon, MCMB, polyacrylonitrile, stearic acid, ascorbic acid, PPy, Super P, polyaniline, soluble starch, cellulose, and sucrose; More preferably, the iron source is one or more of ferrous oxalate, ferric nitrate, iron powder, ferric phosphate, ferrous citrate, ferrous acetate, ferrous formate, ferric pyrophosphate, ferrous pyrophosphate, ferrous phosphate, ferrous oxide, and ferrous oxide. More preferably, the medium solution includes one or more of water, anhydrous ethanol, and ethylene glycol solution.
4. The method for preparing the carbon-coated phosphate iron pyrophosphate precursor material according to any one of claims 1 to 3, characterized in that: In step 1, the solid content of the slurry A is 30% to 70%.
5. The method for preparing the carbon-coated ferric phosphate pyrophosphate precursor material according to any one of claims 1 to 4, characterized in that: In step 3, the calcination temperature is 350-900° C. and the calcination time is 4-20 hours.
6. A carbon-coated iron phosphate pyrophosphate precursor material, characterized in that: It is prepared by the preparation method of the carbon-coated phosphate iron pyrophosphate precursor material according to any one of claims 1 to 5; the carbon content in the phosphate iron pyrophosphate precursor material is 0.2% to 12%.
7. The iron phosphate pyrophosphate precursor material according to claim 6, characterized in that: Particle size D50 is 3.24~4.75μm; specific surface area is 12~16m 2 / g; tap density is 1.4~1.7g / cm 3 .
8. A sodium iron pyrophosphate material, characterized in that: The method is prepared by mixing the carbon-coated phosphate iron pyrophosphate precursor material according to any one of claims 6 to 7 and a sodium source, and calcining the mixture under an inert protective gas.
9. The method for preparing the sodium iron phosphate pyrophosphate material according to claim 8, characterized in that: The sodium source is one or more of sodium carbonate, sodium hydroxide, sodium pyrophosphate, sodium bicarbonate, sodium dihydrogen phosphate, disodium hydrogen phosphate, sodium phosphate, sodium acetate, and sodium oxalate; further preferably, the mass ratio of the phosphate iron pyrophosphate precursor material to the sodium source is 1:0.14~0.98; further preferably, the calcination temperature is 350~1000°C and the calcination time is 4~12h.
10. A sodium ion battery, characterized in that: The positive electrode material is prepared by the preparation method of the carbon-coated sodium iron phosphate pyrophosphate material according to any one of claims 8 to 9.
Citation Information
Patent Citations
Preparation method of sodium ferric manganese phosphate pyrophosphate positive electrode material with core-shell structure
CN116924371A
Preparation method and application of composite phosphoric acid and pyrophosphoric acid polyanionic positive electrode material
CN117361482A
Preparation method for lithium iron phosphate with improved low-temperature performance
CN109607505A
Preparation method and application of ferric sodium pyrophosphate positive electrode material
CN117819512A
Multi-carbon coated ferric sodium pyrophosphate, multi-carbon coated ferric sodium pyrophosphate and sodium ion battery
CN117886295A
Cited By
High-capacity lithium iron manganese phosphate positive electrode material, preparation method thereof and lithium battery
CN119370823A
Sodium-ion battery monomer, preparation method thereof, battery device and power utilization device
CN121583993A
High-compaction-density ferric sodium pyrophosphate positive electrode material, preparation method thereof and positive electrode plate
CN121698320A
A high-compaction-density sodium iron phosphate pyrophosphate positive electrode material, a preparation method thereof and a positive electrode plate
CN121698320B
High-compaction iron phosphate, preparation method thereof and lithium iron phosphate
CN121849883A