A manganese-based Prussian blue cathode material, its preparation method and application

By controlling the formation rate of Mn2+ and reducing the generation of vacancies and coordinated water, the crystallinity and cycle stability of the manganese-based Prussian blue cathode material are improved, the problems of structural stability and poor conductivity are solved, and high specific capacity and good performance are achieved. rate performance.

CN116282073BActive Publication Date: 2024-10-15GUANGDONG BRUNP RECYCLING TECH CO LTD +1
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202310045867.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-01-30
Publication Date
2024-10-15
Estimated Expiration
2043-01-30

AI Technical Summary

Technical Problem

Manganese-based Prussian blue analogues have poor structural stability and conductivity in sodium-ion battery cathode materials, resulting in limited rate performance and power output. This is mainly due to the increased water absorption due to the presence of coordinated water and vacancies, which affects the insertion and extraction of sodium ions. process.

Method used

By adding high-priced solid manganese particles and reducing agents into the Na4Fe(CN)6 solution in small amounts and multiple times, the formation rate of Mn2+ is regulated, the reaction rate is controlled, the generation of vacancies and coordination water is reduced, and the crystallinity and cycle stability of the material are improved.

Benefits of technology

It significantly improves the cycle stability and rate performance of manganese-based Prussian blue cathode materials, ensures high specific capacity and good sodium ion diffusion channel continuity, and improves the transfer rate of sodium ions and the overall performance of the electrode material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004055391850000081
    Figure BDA0004055391850000081
Patent Text Reader

Abstract

The present invention provides a manganese-based Prussian blue positive electrode material and a preparation method and application thereof. The preparation method comprises the following steps: (1) adding a reducing agent solution and solid manganese particles into a sodium ferrocyanide solution for reaction; (2) aging the reactant obtained in step (1), filtering to obtain the manganese-based Prussian blue positive electrode material. The method of the present invention can control the composition of the generated Prussian blue material, so that when the Prussian blue material is used as a positive electrode material for a sodium ion battery, the sodium ion battery has a higher initial Na + content, good stability and rate performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of sodium ion batteries and relates to a manganese-based Prussian blue positive electrode material and a preparation method and application thereof. Background Art

[0002] As lithium-ion batteries enter the field of electric vehicles and large-scale energy storage, their market share has soared due to their advantages such as high energy density, long service life, high charging efficiency and good safety. However, the rapid growth in demand for lithium-ion batteries has led to high lithium resource costs. Compared with lithium-ion batteries, sodium-ion batteries have more cost advantages and have been favored in the fields of large-scale energy storage and low-speed electric vehicles.

[0003] Among the many sodium ion cathode materials, manganese-based Prussian blue analogs (Na x M[Fe(CN)6]·z H2O, M=Mn) is very attractive in development and application due to its high voltage platform, high specific capacity, low raw material cost and simple synthesis method. The defect-free manganese-based Prussian blue analogue (Na2Mn[Fe(CN)6]) has a theoretical specific capacity of 170mAh / g and a charge and discharge platform of 3.56V / 3.44V, which is comparable to the lithium iron phosphate positive electrode material in lithium batteries.

[0004] However, during the synthesis process, the rapid precipitation of Prussian blue compounds will produce a large number of ferrocyanide vacancies. In the unit with ferrocyanide vacancies, the transition metal M is coordinated with five adjacent N ligands, and the remaining one is replaced by water to form coordinated water. The coordinated water will then form hydrogen bonds with the crystal water in the pores of the crystal structure of the Prussian blue cathode material, making the material more hygroscopic. The presence of coordinated water and vacancies reduces the structural stability and conductivity of the Prussian blue analog electrode material during the sodium ion insertion and extraction process, affects its rate performance and power output, and severely limits the application of Prussian blue analogs in sodium ion battery cathode materials.

[0005] CN115367772A discloses a method for preparing a Prussian blue cathode material, which adopts a high-speed shearing method to replace the traditional magnetic stirring or mechanical stirring method, so that the entire reaction system in the coprecipitation process is as close to the ideal reaction state as possible, and each ion is evenly dispersed in the solution and complexed with each other at the same probability; at the same time, the coprecipitation and aging process is temperature-controlled to regulate the grain nucleation growth process, so as to obtain a Prussian blue cathode material with high crystallinity, low defects, low water content and high sodium content.

[0006] CN106920964A discloses a transition metal element gradient substituted Prussian blue type sodium ion battery positive electrode material and a preparation method thereof, wherein the preparation method comprises the following steps: firstly, sodium ferrocyanide, ferrous chloride, and a mixture of a substitution element chloride and ferrous chloride are respectively dissolved in deionized water to obtain respective precursor solutions; then, a Prussian blue suspension in which the substitution element is distributed in a concentration gradient from the inside to the surface of the grain is obtained through a coprecipitation reaction; and after centrifugation, washing, and vacuum drying, the material is prepared.

[0007] The above method mainly adopts a co-precipitation method to mix a Na4Fe(CN)6 solution with a transition metal salt solution to prepare a Prussian blue material. This method has a fast reaction rate and is prone to produce a large number of vacancies, crystal water and coordinated water inside. Summary of the invention

[0008] The object of the present invention is to provide a manganese-based Prussian blue positive electrode material and a preparation method and application thereof. The method of the present invention is to add high-valent solid manganese particles and a reducing agent in small amounts and multiple times into a Na4Fe(CN)6 solution to control the Mn 2+ The formation rate of the cathode material is controlled by the method, which can significantly improve the crystallinity of the material and effectively improve the cycle stability and rate performance of the cathode material.

[0009] In order to achieve the purpose of the invention, the present invention adopts the following technical solutions:

[0010] In a first aspect, the present invention provides a method for preparing a manganese-based Prussian blue positive electrode material, the preparation method comprising the following steps:

[0011] (1) adding a reducing agent solution and solid manganese particles into a sodium ferrocyanide solution to react;

[0012] (2) The reactant obtained in step (1) is aged and then filtered to obtain the manganese-based Prussian blue positive electrode material.

[0013] In the present invention, high-valent solid manganese particles and a reducing agent are first added to a sodium ferrocyanide solution in small amounts and multiple times, and the reducing agent reduces the high-valent solid manganese source to form Mn 2+ , then the formed Mn 2+ It reacts with Na4Fe(CN)6 in the reaction system to slowly form a precipitate. Then, by controlling the concentration of the reducing agent and the amount of high-valent solid manganese particles, the Mn 2+The formation rate of the reaction rate is controlled. This slow reaction greatly improves the crystallinity of the material and reduces the generation of vacancies and the introduction of coordinated water and crystallization water. The reduction of vacancies ensures that the material has sufficient redox active sites and the electrode material has a high specific capacity. At the same time, the low vacancy content ensures the continuity of the sodium ion diffusion channel, which makes the electrode material have good rate characteristics. The reduction of coordinated water and structural water can reduce the negative reaction of water with sodium ions and positive electrode materials during the cycle, thereby improving the cycle stability. At the same time, reducing the storage sites occupied by interstitial water can increase the transfer rate of sodium ions and improve the rate performance.

[0014] Preferably, the reducing agent solution in step (1) comprises ascorbic acid solution and / or citric acid solution.

[0015] Preferably, the volume of the reducing agent solution is 80-120 mL.

[0016] Preferably, the mass concentration of the ascorbic acid solution is 50-100 g / L, for example, 50 g / L, 60 g / L, 70 g / L, 80 g / L, 90 g / L or 100 g / L.

[0017] Preferably, the molar concentration of the citric acid solution is 0.2-0.5 mol / L, for example, 0.2 mol / L, 0.25 mol / L, 0.3 mol / L, 0.4 mol / L or 0.5 mol / L.

[0018] Preferably, the adding rate of the reducing agent solution in step (1) is 8 to 12 mL / h, for example, 8 mL / h, 9 mL / h, 10 mL / h, 11 mL / h or 12 mL / h.

[0019] Preferably, the solid manganese in step (1) comprises a manganese-containing compound with a manganese valence of ≤4 which is unreactive under the condition of pH = 4.5.

[0020] Preferably, the solid manganese includes any one of dimanganese trioxide, manganese dioxide or trimanganese tetroxide, or a combination of at least two thereof.

[0021] Preferably, the median particle size D50 of the solid manganese particles is 150-300 nm, for example, 150 nm, 180 nm, 200 nm, 250 nm or 300 nm.

[0022] Preferably, the solid manganese particles are added to the sodium ferrocyanide solution in 8 to 12 times (eg 8 times, 9 times, 10 times, 11 times or 12 times, etc.).

[0023] Preferably, the solid manganese particles are added at a frequency of 1 time / h.

[0024] Preferably, the solid manganese particles are added at a rate of 0.13 to 0.18 g / time, for example, 0.13 g / time, 0.14 g / time, 0.15 g / time, 0.16 g / time or 0.18 g / time.

[0025] Preferably, the mass concentration of the sodium ferrocyanide solution in step (1) is 40-60 g / L, for example: 40 g / L, 45 g / L, 50 g / L, 55 g / L or 60 g / L.

[0026] Preferably, the mass ratio of the solid manganese particles to sodium ferrocyanide is (1-5):10, for example: 1:10, 1.2:10, 3:10, 4:10 or 5:10, etc.

[0027] Preferably, the reaction temperature in step (1) is 50-80°C, for example, 50°C, 55°C, 60°C, 70°C or 80°C.

[0028] Preferably, the reaction time is 8 to 12 hours, for example, 8 hours, 9 hours, 10 hours, 11 hours or 12 hours.

[0029] Preferably, the aging time in step (2) is 10 to 15 hours, for example: 10 hours, 11 hours, 12 hours, 13 hours, 14 hours or 15 hours, etc.

[0030] Preferably, the filtration in step (2) is followed by washing and vacuum drying.

[0031] Preferably, the vacuum drying temperature is 100-120°C, for example, 100°C, 105°C, 110°C, 115°C or 120°C.

[0032] Preferably, the vacuum drying time is 8 to 15 hours, for example, 8 hours, 9 hours, 10 hours, 12 hours or 15 hours.

[0033] In a second aspect, the present invention provides a manganese-based Prussian blue positive electrode material, wherein the manganese-based Prussian blue positive electrode material is prepared by the method described in the first aspect.

[0034] In a third aspect, the present invention provides a sodium ion battery, wherein the sodium ion battery comprises the manganese-based Prussian blue positive electrode material as described in the second aspect.

[0035] Compared with the prior art, the present invention has the following beneficial effects:

[0036] (1) The method of the present invention can control the composition of the generated Prussian blue material, so that when it is used as a positive electrode material for a sodium ion battery, the sodium ion battery has a higher initial Na + content, good stability and rate performance.

[0037] (2) The battery made of the manganese-based Prussian blue positive electrode material of the present invention has an initial charge and discharge capacity of more than 136.1 mAh / g at 0.1C, an initial charge and discharge capacity of more than 106.4 mAh / g at 5C, and an initial capacity of more than 117.5 mAh / g after 100 cycles. The capacity retention rate after 100 cycles can reach more than 86%. DETAILED DESCRIPTION

[0038] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.

[0039] Example 1

[0040] This embodiment provides a manganese-based Prussian blue positive electrode material, and the preparation method of the manganese-based Prussian blue positive electrode material is as follows:

[0041] (1) 9.86 g Na4Fe(CN)6·10H2O was dissolved in 200 mL of deionized water, and 8 g of ascorbic acid was dissolved in 100 mL of deionized water. The mixture was stirred and then 1.58 g of Mn2O3 black solid particles (average particle size 200 nm) and ascorbic acid solution were slowly added to the sodium ferrocyanide solution at 60°C. The solid particles were added once per hour, 0.158 g each time, and the ascorbic acid solution was added at a rate of 10 mL / h. The reaction was continued for 10 h.

[0042] (2) The reactant obtained in step (1) is aged for 11 hours, and the precipitate is collected by centrifugation, then washed, and dried in a vacuum drying oven at 115° C. for 11 hours to obtain the manganese-based Prussian blue material.

[0043] Example 2

[0044] This embodiment provides a manganese-based Prussian blue positive electrode material, and the preparation method of the manganese-based Prussian blue positive electrode material is as follows:

[0045] (1) 9.86 g Na4Fe(CN)6·10H2O was dissolved in 200 mL deionized water and stirred. At 60°C, 1.58 g Mn2O3 black solid particles (average particle size 200 nm) and 100 mL 0.4 mol / L citric acid solution were slowly added to the sodium ferrocyanide solution. The solid particles were added once per hour, 0.158 g each time, and the sodium citrate solution was added at a rate of 10 mL / h. The reaction was continued for 10 h.

[0046] (2) The reactant obtained in step (1) is aged for 12 hours, and the precipitate is collected by centrifugation, then washed, and dried in a vacuum drying oven at 110° C. for 10 hours to obtain the manganese-based Prussian blue material.

[0047] Example 3

[0048] The only difference between this embodiment and embodiment 1 is that the mass concentration of the ascorbic acid solution is 30 g / L, and the other conditions and parameters are exactly the same as those in embodiment 1.

[0049] Example 4

[0050] The only difference between this embodiment and embodiment 1 is that the mass concentration of the ascorbic acid solution is 120 g / L, and the other conditions and parameters are exactly the same as those in embodiment 1.

[0051] Example 5

[0052] The only difference between this embodiment and embodiment 2 is that the molar concentration of the citric acid solution is 0.1 mol / L, and the other conditions and parameters are exactly the same as those in embodiment 1.

[0053] Example 6

[0054] The only difference between this embodiment and embodiment 2 is that the molar concentration of the citric acid solution is 0.6 mol / L, and the other conditions and parameters are exactly the same as those in embodiment 1.

[0055] Example 7

[0056] The only difference between this embodiment and embodiment 1 is that the mass of Mn2O3 added each time is 0.12 g, and the other conditions and parameters are exactly the same as those in embodiment 1.

[0057] Example 8

[0058] The only difference between this embodiment and embodiment 1 is that the mass of Mn2O3 added each time is 0.2 g, and the other conditions and parameters are exactly the same as those in embodiment 1.

[0059] Comparative Example 1

[0060] This comparative example provides a manganese-based Prussian blue positive electrode material, and the preparation method of the manganese-based Prussian blue positive electrode material is as follows:

[0061] 9.86 g Na4Fe(CN)6·10H2O was dissolved in 200 mL deionized water; 1.52 g MnSO4 was dissolved in 100 mL deionized water, and the mixture was stirred to obtain a solution with a MnSO4 concentration of 0.1 mol / L; the MnSO4 solution was added dropwise to the Na4Fe(CN)6 solution under stirring at 60°C, and then aged for 12 hours. The precipitate was collected by centrifugation, washed, and dried in a vacuum drying oven at 110°C for 10 hours to obtain a manganese-based Prussian blue material.

[0062] Comparative Example 2

[0063] This comparative example provides a manganese-based Prussian blue positive electrode material, and the preparation method of the manganese-based Prussian blue positive electrode material is as follows:

[0064] 9.86 g of Na4Fe(CN)6·10H2O was dissolved in 200 mL of deionized water; 1.52 g of MnSO4 was dissolved in 100 mL of deionized water, and after stirring, a solution with a MnSO4 concentration of 0.1 mol / L was obtained, and then 100 mL of 0.1 mol / L sodium citrate solution was added; at 60° C., the above solution was added dropwise to the Na4Fe(CN)6 solution under stirring, and then the aging was continued for 12 hours, and the precipitate was collected by centrifugation, and then washed and dried in a vacuum drying oven at 110° C. for 10 hours to obtain a manganese-based Prussian blue material.

[0065] Performance Test:

[0066] The powder materials obtained in the examples and comparative examples were homogenized in a ratio of active component: PVDF: conductive agent = 7:1:2 to prepare 2025 button batteries. Electrochemical tests were performed at 4.0-2.5V and 0.1C. The test results are shown in Table 1:

[0067] Table 1

[0068]

[0069] As can be seen from Table 1, from Examples 1-2, the manganese-based Prussian blue positive electrode material of the present invention can produce a battery with a 0.1C first charge and discharge specific capacity of more than 136.1 mAh / g, a 5C first charge and discharge specific capacity of more than 106.4 mAh / g, a specific capacity of more than 117.5 mAh / g after 100 cycles, and a capacity retention rate of more than 86% after 100 cycles.

[0070] By comparing Example 1 with Example 3-4, and Example 2 with Example 5-6, it can be seen that the concentration of the reducing agent solution used in the present invention will affect the performance of the obtained manganese-based Prussian blue positive electrode material. The mass concentration of the ascorbic acid solution is controlled at 50-100 g / L, and the molar concentration of the citric acid solution is controlled at 0.2-0.5 mol / L. The performance of the manganese-based Prussian blue positive electrode material is better. If the concentration of the reducing agent solution is too high, the reaction rate will be too fast. If the concentration of the reducing agent solution is too low, Mn 2+ The restoration effect is poor.

[0071] By comparing Example 1 with Examples 7-8, it can be seen that the mass of solid manganese particles added each time will affect the performance of the manganese-based Prussian blue positive electrode material. When the addition rate of the solid manganese particles is controlled at 0.13-0.18 g / time, the performance of the manganese-based Prussian blue positive electrode material is better. If the addition rate of the solid manganese particles is too fast, the reaction rate cannot be reduced. If the addition rate of the solid manganese particles is too slow, the effect will be significantly worse.

[0072] From the comparison between Example 1 and Comparative Examples 1-2, it can be seen that the present invention controls the Mn by controlling the dropwise concentration of the reducing agent and the amount of the high-valent solid manganese particles. 2+ The formation rate is controlled to achieve the control of the reaction rate. This slow reaction greatly improves the crystallinity of the material, reduces the generation of vacancies and the introduction of coordinated water and crystallization water, improves its rate performance and stable cyclicity, and achieves an effect better than the method of adding a complexing agent in Comparative Example 2.

[0073] The applicant declares that the above is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily thought of by those skilled in the art within the technical scope disclosed by the present invention shall fall within the protection scope and disclosure scope of the present invention.

Claims

1. A method for preparing a manganese-based Prussian blue positive electrode material, It is characterized in that The preparation method comprises the following steps: (1) adding a reducing agent solution and solid manganese particles into a sodium ferrocyanide solution for reaction; The solid manganese comprises any one of dimanganese trioxide, manganese dioxide or trimanganese tetraoxide, or a combination of at least two thereof; The solid manganese particles are added at a frequency of 1 time / h; The solid manganese particles are added at a rate of 0.13-0.18 g / time; The adding rate of the reducing agent solution is 8-12 mL / h; (2) The reactant obtained in step (1) is aged and then filtered to obtain the manganese-based Prussian blue positive electrode material.

2. The preparation method according to claim 1, It is characterized in that The reducing agent solution in step (1) includes ascorbic acid solution and / or citric acid solution.

3. The preparation method according to claim 1, It is characterized in that The volume of the reducing agent solution is 80-120 mL.

4. The preparation method according to claim 2, It is characterized in that The mass concentration of the ascorbic acid solution is 50-100 g / L.

5. The preparation method according to claim 2, It is characterized in that The molar concentration of the citric acid solution is 0.2-0.5 mol / L.

6. The preparation method according to claim 1, It is characterized in that The median particle size D50 of the solid manganese particles is 150-300 nm.

7. The preparation method according to claim 1, It is characterized in that The solid manganese particles are added into the sodium ferrocyanide solution in 8 to 12 times.

8. The preparation method according to claim 1, It is characterized in that The mass concentration of the sodium ferrocyanide solution in step (1) is 40-60 g / L.

9. The preparation method according to claim 1, It is characterized in that The mass ratio of the solid manganese particles to sodium ferrocyanide is (1-5):

10.

10. The preparation method according to claim 1, It is characterized in that The reaction temperature in step (1) is 50-80°C.

11. The preparation method according to claim 1, It is characterized in that The reaction time is 8 to 12 hours.

12. The preparation method according to claim 1, It is characterized in that The aging time in step (2) is 10 to 15 hours.

13. The preparation method according to claim 1, It is characterized in that The filtration in step (2) is followed by washing and vacuum drying.

14. The preparation method according to claim 13, It is characterized in that The vacuum drying temperature is 100-120°C.

15. The preparation method according to claim 13, It is characterized in that The vacuum drying time is 8 to 15 hours.

16. A manganese-based Prussian blue positive electrode material, It is characterized in that The manganese-based Prussian blue positive electrode material is prepared by the method for preparing the manganese-based Prussian blue positive electrode material as claimed in any one of claims 1 to 15.

17. A sodium ion battery, It is characterized in that The sodium ion battery comprises the manganese-based Prussian blue positive electrode material as claimed in claim 16.

Citation Information

Cited By

  • Manganese-based Prussian blue analogue positive electrode for sodium ion battery and preparation method of manganese-based Prussian blue analogue positive electrode

    CN120089690A