A method for preparing high entropy oxide material based on natural minerals, high entropy oxide material and application thereof

Preparation of high-entropy oxide materials through natural mineral calcination and sintering has solved the problems of high cost and impurity phases in the prior art, and achieved high-purity and high-performance electrode materials production, suitable for lithium-ion and sodium-ion batteries.

CN116282238BActive Publication Date: 2024-12-03CENT SOUTH UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211092957.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-09-08
Publication Date
2024-12-03
Estimated Expiration
2042-09-08

AI Technical Summary

Technical Problem

The existing high entropy oxide electrode materials are costly to produce and often contain impurity phases in the materials, which affects electrochemical stability and performance.

Method used

Natural minerals are used as raw materials, and sintered after calcination, crushing, mixing and processing with lithium or sodium sources to directly prepare high-entropy oxide materials, eliminating smelting and synthesis steps, simplifying the process flow, and reducing costs.

Benefits of technology

It obtains high-entropy oxide materials with high purity and no impurity phases, which have excellent electrochemical activity and rate performance, and are suitable for electrochemical energy storage devices such as lithium ion and sodium ion batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116282238B_ABST
    Figure CN116282238B_ABST
Patent Text Reader

Abstract

The present invention provides a method for preparing a high entropy oxide material based on natural minerals, a high entropy oxide material and its application. The structural formula of the high entropy oxide material is: x (M 1 M 2 M 3 …M n ) 2‑x O 2 , where A is Na or Li, 0.8<x<1.5, n≥5, M 1 、M 2 、M 3 ,…M n Respectively represent different metal ions; the method comprises the following steps: fully calcining natural mineral concentrates containing corresponding metal elements in air to obtain calcined products; fully mixing the calcined products with lithium source or sodium source powder according to a stoichiometric ratio, and then pressing tablets, and sintering in an air atmosphere or an inert atmosphere to obtain a high-entropy oxide material; the natural mineral concentrate is a concentrate with a purity of ≥95%; the calcination temperature is 600-1200°C; the present invention reduces the production cost of high-entropy electrode materials, and the obtained high-entropy oxide material has high purity, does not contain impurity phases, and has a stable crystal structure.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of electrode materials, and more specifically, to a method for preparing a high entropy oxide material based on natural minerals, a high entropy oxide material and applications thereof. Background Art

[0002] High entropy materials are a type of new material with a single phase structure that has been proposed in recent years. It is obtained by solid dissolving 5 or more metal or non-metal compounds. It has unique composition, configuration and adjustable performance. Electrode materials under the high entropy strategy show a trend of performance enhancement and can be used to effectively design and develop various high-performance electrode materials. The entropy-driven structural stability can improve the electrochemical stability of electrode materials. The unique hysteresis diffusion effect of high entropy can slow down the agglomeration of secondary particles during the cycle, which is beneficial to improving the structural stability and integrity of electrode materials. The lattice distortion effect and the electronic structure diversity of high entropy components can improve the conductivity of electrode materials and increase the carrier diffusion rate, which is beneficial to improving the rate performance of electrode materials.

[0003] Therefore, the introduction of high entropy design concepts will greatly expand the design space of secondary ion battery electrode materials and bring new opportunities to break through the current bottlenecks in sodium ion battery performance and commercial applications. For example, Hu Yongsheng et al. reported an O3-type layered high entropy oxide NaNi 0.12 Cu 0.12 Mg 0.12 Fe 0.15 Co 0.15 Mn 0.1 Ti 0.12 Sn 0.1 Sb 0.04 O2, the material has good cycle stability, and provides a feasible idea and reference for the research of high entropy layered oxide materials. However, NiO, CuO, MgO, Fe2O3, Co2O3, MnO2, TiO2, SnO2, Sb2O5, etc. selected by this method are all industrial products with high prices, which increases the material production cost. Summary of the invention

[0004] Based on the above technical problems existing in the prior art, one of the objects of the present invention is to provide a method for preparing high entropy oxide materials based on natural minerals. This method uses natural minerals as raw materials, which are directly used as precursor materials of high entropy oxide materials after simple processing, thereby eliminating the steps of smelting, synthesizing reagents, and preparing materials. This not only shortens the production process and reduces pollution, but also directly reduces the production cost of high entropy electrode materials. The obtained high entropy oxide has high purity, does not contain impurity phases, and has a stable crystal structure.

[0005] In order to achieve the above object, the technical solution of the present invention is as follows:

[0006] A method for preparing a high entropy oxide material based on natural minerals, wherein the high entropy oxide material has the structural formula: A x (M1M2M3…M n ) 2-x O2, wherein A is Na or Li, 0.8<x<1.5, n≥5, M1, M2, M3, ...M n Respectively represent different metal ions, the metal ions include Zr 4+ , Mn 2+ , Mn 3+ , Mn 4+ , Fe 2+ , Fe 3+ 、Zn 2+ 、Cd 2+ , Hg 2+ 、Ag + 、Mo 2+ 、Mo 3+ 、Ru 4+ 、Ru 5+ , Ir 4+ , Ir 5+ , Rh 4+ 、Mo 6+ 、V 5+ , Nb 5+ 、Ti 4+ Sn 4+ , Sb 5+ Cr 3+ Cr 6+ 、Ni 2+ 、Ni 3+ 、Co 2+ 、Co 3+ , Cu 2+ At least 5 of the above; the method comprises the following steps:

[0007] S1. Fully calcining the natural mineral concentrates containing the corresponding metal elements in air, and crushing them to obtain calcined products;

[0008] S2, fully mixing the calcined product with lithium source or sodium source powder according to a stoichiometric ratio to obtain a precursor powder;

[0009] S3, pressing the precursor into tablets, sintering in an air atmosphere or an inert atmosphere, and cooling to obtain the high entropy oxide material;

[0010] The natural mineral concentrate is a concentrate with a purity of ≥95%; in step S1, the calcination temperature is 600-1200°C.

[0011] It should be noted that the natural mineral concentrate refers to a natural element or compound formed under geological action, which has a unique chemical composition expressed by a chemical formula and a relatively fixed chemical composition, and has a purity of ≥95% after being processed by modern technology.

[0012] In some embodiments, the calcination time is 5 to 10 hours to ensure complete conversion of the concentrate.

[0013] In some embodiments, in step S3, the sintering process is: firstly heating to 300-600°C for pre-sintering, and then heating to 800-1000°C for sintering.

[0014] In some embodiments, the pre-sintering time at 300-600° C. is 3-5 h; and the sintering time at 800-1000° C. is 6-12 h.

[0015] In some embodiments, in step S3, the heating rates of the pre-sintering and sintering processes are both 3-5°C / min.

[0016] In some embodiments, in step S2, the calcined product and the lithium source or sodium source are mixed, ball-milled, and then ethanol or acetone is added to form a slurry, which is then ball-milled again, and finally dried to obtain the precursor powder.

[0017] In some embodiments, in step S2, the lithium source is at least one of lithium hydroxide, lithium carbonate, and lithium oxide; the sodium source is at least one of sodium hydroxide and sodium carbonate. The lithium source or sodium source is added in excess of 5-10wt% to compensate for the loss during high-temperature sintering.

[0018] A second object of the present invention is to provide a high entropy oxide material, which is made by the method of any of the above-mentioned embodiments.

[0019] A third object of the present invention is to provide a positive electrode active material, wherein the positive electrode active material comprises the above-mentioned high entropy oxide material.

[0020] A fourth object of the present invention is to provide a positive electrode, which includes the above-mentioned positive electrode active material.

[0021] A fifth object of the present invention is to provide an electrochemical energy storage device, the electrochemical energy storage device comprising the above-mentioned positive electrode. Specifically, the electrochemical energy storage device is a lithium ion secondary battery, a sodium ion secondary battery or a capacitor.

[0022] Compared with the prior art, the present invention has the following beneficial effects:

[0023] The present invention uses natural mineral concentrate as raw material, calcines them separately at a specific temperature, then mixes them according to a stoichiometric ratio and sinters them with a lithium source or a sodium source to obtain a high entropy oxide material, thereby eliminating the steps of smelting, synthetic reagents, material preparation, etc., simplifying the preparation process, shortening the production process, and the raw materials are cheap and easily available, which greatly reduces the production cost.

[0024] The high entropy oxide material obtained by the method of the present invention has high purity, does not contain impurity phases, and has a stable crystal structure. The high entropy oxide material has high electrochemical activity and is applied as a positive electrode active material in an electrochemical energy storage device (such as a lithium ion battery, a sodium ion battery, a capacitor, etc.) to exhibit high operating voltage, excellent rate performance and cycle performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 is a process flow chart of the present invention;

[0026] Figure 2 The high entropy oxide material Na(Ni 1 / 6 Cu 1 / 6 Fe 1 / 6 Mn 1 / 6 Sn 1 / 6 Ti 1 / 6 )XRD pattern of O2;

[0027] Figure 3 The high entropy oxide material Na(Ni 1 / 6 Cu 1 / 6 Fe 1 / 6 Mn 1 / 6 Sn 1 / 6 Ti 1 / 6 ) SEM image of O2;

[0028] Figure 4 The high entropy oxide material Na(Ni 1 / 6 Cu 1 / 6 Fe 1 / 6 Mn 1 / 6 Sn 1 / 6 Ti 1 / 6 )O2 first cycle charge and discharge curve;

[0029] Figure 5 is the high entropy oxide material Li in Example 2 1.2 (Ni 2 / 15 Mn 2 / 15 Cr 2 / 15 Ti 2 / 15 Mo 2 / 15 Nb 2 / 15 )XRD pattern of O2;

[0030] Figure 6is the high entropy oxide material Li in Example 2 1.2 (Ni 2 / 15 Mn 2 / 15 Cr 2 / 15 Ti 2 / 15 Mo 2 / 15 Nb 2 / 15 ) SEM image of O2;

[0031] Figure 7 is the Li of the high entropy oxide material in Example 2 1.2 (Ni 2 / 15 Mn 2 / 15 Cr 2 / 15 Ti 2 / 15 Mo 2 / 15 Nb 2 / 15 )O2 first cycle charge and discharge curve. DETAILED DESCRIPTION

[0032] Many specific details are set forth in the following description to facilitate a full understanding of the present invention. However, the present invention can be implemented in many other ways than those described herein, and those skilled in the art can make similar modifications without violating the connotation of the present invention, so the present invention is not limited to the specific implementation disclosed below.

[0033] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used in the specification of the present invention herein are only for the purpose of describing specific embodiments and are not intended to limit the present invention.

[0034] Example 1

[0035] This embodiment provides a high entropy oxide material prepared from natural minerals, whose molecular formula is Na(Ni 1 / 6Cu 1 / 6 Fe 1 / 6 Mn 1 / 6 Sn 1 / 6 Ti 1 / 6 )O2, its preparation process is as follows Figure 1 As shown, the specific steps include:

[0036] Step S1, using pentlandite, chalcopyrite, pyrolusite, stannite and rutile with purity greater than 95% as raw materials, calcining them in an air atmosphere at 900° C. for 10 hours, and then crushing the calcined products to obtain calcined product powders;

[0037] Step S2, mixing the calcined product powder according to a stoichiometric ratio and mixing with a corresponding stoichiometric amount of sodium carbonate, wherein the sodium carbonate is in excess of 5 wt% to prevent loss during high temperature treatment;

[0038] Step S3, adding ethanol to prepare a precursor slurry, and then using a ball milling method to mix the precursor slurry evenly, with a ball-to-material ratio of 10:1, a ball milling time of 12 hours, and a rotation speed of 500r / min; then drying at 60°C to 80°C for 8 hours to obtain a precursor powder;

[0039] Step S4, pressing the precursor under a pressure of 10 to 15 MPa, and then placing it in a tubular heating furnace or a muffle furnace, sintering it in an air atmosphere, and naturally cooling it after high-temperature sintering to obtain a product; wherein the high-temperature sintering is carried out in two stages, wherein the first stage is pre-sintering, heating the temperature to 600°C at a heating rate of 3°C / min and pre-sintering for 5 hours, and then heating the temperature to 1000°C at a heating rate of 4°C / min for the second stage of high-temperature sintering, and the sintering time is 10 hours;

[0040] Step S5: Grind the product thoroughly to obtain a high entropy oxide material Na(Ni 1 / 6 Cu 1 / 6 Fe 1 / 6 Mn 1 / 6 Sn 1 / 6 Ti 1 / 6 )O2.

[0041] The obtained XRD patterns of high entropy oxide materials can be found in Figure 2 The XRD spectrum shows that its structure is an O3 layered structure, the space point group is R-3m, and there is no impurity phase; its SEM picture is as follows Figure 3 As shown, the particle size of the material after grinding is between 2 and 5 microns, and the grain distribution range is relatively concentrated.

[0042] The high entropy oxide material Na(Ni 1 / 6 Cu 1 / 6 Fe 1 / 6 Mn 1 / 6 Sn 1 / 6 Ti 1 / 6 )O2 is used as the positive electrode active material of the sodium ion secondary battery to make the positive electrode sheet. The specific method is: the prepared Na(Ni 1 / 6 Cu 1 / 6 Fe 1 / 6 Mn 1 / 6Sn 1 / 6 Ti 1 / 6 )O2 powder was mixed with acetylene black and polyvinylidene fluoride (PVDF, adhesive) in a mass ratio of 80:10:10, and an appropriate amount of N-methylpyrrolidone (NMP) solution was added as a dispersant. The mixture was magnetically stirred for 3 h to prepare a slurry. The slurry was then coated on an aluminum foil current collector, dried under vacuum at 120°C for 8 h, and transferred to an Ar atmosphere glove box for use.

[0043] The half-cell was assembled in an Ar atmosphere glove box, with sodium metal as the counter electrode and NaPF6 / ethylene carbonate (EC:DMC:DEC=1:1:1) solution as the electrolyte, and assembled into a CR2016 button cell. The charge and discharge test was carried out at a current density of C / 10 (12mA / g) using a constant current charge and discharge mode, with the charge cutoff voltage set to 4.3V and the discharge cutoff voltage set to 2.0V. The first cycle charge and discharge curve is shown in Figure 2. Figure 4 As shown, the discharge specific capacity is 89.5354 mAh / g and the first-cycle coulombic efficiency is 91.54%.

[0044] Example 2

[0045] This embodiment provides a high entropy oxide material prepared from natural minerals, whose chemical formula is Li 1.2 (Ni 2 / 15 Mn 2 / 15 Fe 2 / 15 Ti 2 / 15 Mo 2 / 15 Nb 2 / 15 )O2, the preparation process of the high entropy oxide material is as follows Figure 1 As shown, the specific steps include:

[0046] Step S1, using laterite nickel ore, pyrolusite, rutile, molybdenite and columbite with purity greater than 95% as raw materials, respectively, calcining them in an air atmosphere at 900° C. for 10 hours, and then crushing the calcined products to obtain calcined product powders;

[0047] Step S2, mixing the calcined product powder according to a stoichiometric ratio and mixing with a corresponding stoichiometric amount of lithium carbonate, wherein the lithium carbonate is in excess of 5 wt% to prevent loss during high temperature treatment;

[0048] Step S3, adding ethanol to prepare a precursor slurry, and then using a ball milling method to mix the precursor slurry evenly, with a ball-to-material ratio of 10:1, a ball milling time of 12 hours, and a rotation speed of 500r / min; then drying at 60°C to 80°C for 8 hours to obtain a precursor powder;

[0049] Step S4, pressing the precursor under a pressure of 10 to 15 MPa, and then placing it in a tubular heating furnace or a muffle furnace, sintering it in an air atmosphere, and naturally cooling it after high-temperature sintering to obtain a product; wherein the high-temperature sintering is carried out in two stages, wherein the first stage is pre-sintering, heating the temperature to 600°C at a heating rate of 3°C / min and pre-sintering for 5 hours, and then heating the temperature to 1000°C at a heating rate of 4°C / min for the second stage of high-temperature sintering, and the sintering time is 10 hours;

[0050] Step S5: Grind the product thoroughly to obtain a high entropy oxide material Na(Ni1 / 6 Cu 1 / 6 Fe 1 / 6 Mn 1 / 6 Sn 1 / 6 Ti 1 / 6 )O2.

[0051] The XRD spectrum of the high entropy oxide material obtained in this example can be found in Figure 5 The XRD spectrum shows that the obtained high entropy oxide material has a Fm-3m structure, and its SEM image is as follows Figure 6 shown.

[0052] The high entropy oxide material Li prepared in this embodiment 1.2 (Ni 2 / 15 Mn 2 / 15 Fe 2 / 15 Ti 2 / 15 Mo 2 / 15 Nb 2 / 15 )O2 is used as the positive electrode active material of lithium-ion secondary batteries, and the positive electrode sheet is made and the lithium-ion half-cell is assembled. The charge and discharge test is carried out at a current density of C / 10 (20mA / g) using the constant current charge and discharge mode. The charge cut-off voltage is set to 4.7V and the discharge cut-off voltage is set to 1.5V. The first cycle charge and discharge curve is as follows Figure 7 As shown, the discharge specific capacity is 233.11 mAh / g and the first-cycle coulombic efficiency is 89.45%.

[0053] The two high entropy oxide materials prepared based on natural minerals in the above embodiments both have high first coulombic efficiency. The results of the embodiments show that the direct conversion of mineral materials to high entropy oxide materials can be achieved through the present invention, which directly reduces the preparation cost of high entropy oxide materials and realizes the short process and efficient value-added of mineral materials. The high entropy stabilization effect enhances the compatibility of elements, so that the prepared high entropy oxide material has a single phase structure without impurity phases. The entropy-driven structural stability improves the electrochemical stability of the electrode material.

[0054] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0055] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.

Claims

1. A method for preparing high entropy oxide materials based on natural minerals, characterized in that: The structure of the high entropy oxide material is an O3 layered structure, the space point group is R-3m, and the chemical formula is: Na(Ni 1 / 6 Cu 1 / 6 Fe 1 / 6 Mn 1 / 6 Sn 1 / 6 Ti 1 / 6 )O2; or, the high entropy oxide material is a Fm-3m type structure, and its chemical formula is: Li 1.2 (Ni 2 / 15 Mn 2 / 15 Cr 2 / 15 Ti 2 / 15 Mo 2 / 15 Nb 2 / 15 )O2; The method comprises the following steps: S1. Fully calcining the natural mineral concentrates containing the corresponding metal elements in air, and crushing them to obtain calcined products; S2, fully mixing the calcined product with lithium source or sodium source powder according to a stoichiometric ratio to obtain a precursor powder; S3, pressing the precursor into tablets, sintering in an air atmosphere or an inert atmosphere, and cooling to obtain the high entropy oxide material; The natural mineral concentrate is a concentrate with a purity of ≥95%; in step S1, the calcination temperature is 600-1200°C; In step S3, the sintering process is: firstly heating to 300-600°C for pre-sintering, and then heating to 800-1000°C for sintering; the heating rates of the pre-sintering and sintering processes are both 3-5°C / min; In step S2, the calcined product and the lithium source or sodium source are mixed, ball-milled, and then ethanol or acetone is added to form a slurry and then ball-milled again, and finally dried to obtain the precursor powder; the lithium source is at least one of lithium hydroxide, lithium carbonate, and lithium oxide; the sodium source is at least one of sodium hydroxide and sodium carbonate.

2. The high entropy oxide material obtained by the preparation method according to claim 1.

3. A positive electrode active material, characterized in that: Comprising the high entropy oxide material as described in claim 2.

4. A positive electrode, characterized in that Comprising the positive electrode active material as claimed in claim 3.

5. An electrochemical energy storage device, characterized in that: Comprising the positive electrode as claimed in claim 4.