Co-doped SrRuO3 material with high coercivity and preparation method thereof
By doping Co elements in SrRuO3 and using the chelation of citric acid solution, the problem of insufficient coercive force of SrRuO3 material is solved, and the preparation of high coercive Co-doped SrRuO3 material is realized, simplifying the preparation process and improving the The stability of the material.
Patent Information
- Application Number
- CN202310207618.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-01
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2043-03-01
AI Technical Summary
The coercive force of SrRuO3 material is low, resulting in poor stability, limiting its further development and application in electronic devices.
By doping Co elements in SrRuO3 and using the carbonyl carboxylic acid in the citric acid solution as a chelating agent, a metal carboxylate complex is formed, atomic doping is achieved, lattice stress is generated, and the coercivity of the material is enhanced. And the grain size is controlled through low-temperature self-combustion reaction to achieve high-temperature sintering.
The coercive force of SrRuO3 material is significantly improved, the controllable adjustment of coercive force is achieved, the preparation process is simplified, the damage to the sample crystal structure is avoided, and the Co-doped SrRuO3 material with excellent performance is obtained.
Smart Images

Figure CN116282239B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of modified perovskite materials, and particularly relates to a Co-doped SrRuO3 material with high coercivity and a preparation method thereof. Background Art
[0002] As a subject widely studied by many scientific researchers, magnetic materials have very important development prospects in the field of spin electronics. With the increase in the integration of electronic devices, entering the post-Moore era and physical devices with high integration, the thermal effect of current cannot be ignored, which seriously restricts the information processing speed and storage density. In order to further improve the information processing speed and storage density, making full use of the spin of electrons is a new way, which can make the electron spin and charge become information carriers together, promoting the miniaturization of electronic devices. Magnetic perovskite materials can combine memory and logic into one device, and have advantages such as fast processing speed and huge magnetoresistance, which has attracted great attention and in-depth research.
[0003] Strontium ruthenate (SrRuO3) is the only oxide with ferromagnetic metallic properties among ABO3-type perovskite 4d transition metals. It has good thermal and chemical stability and is easy to form epitaxial structures with other perovskite structural materials. It has now become a mature electrode material in oxide heterojunctions. However, SrRuO3 has a low coercivity, resulting in poor stability, which hinders its further development and practical application.
[0004] In the prior art, ball milling mixing, epitaxial growth and other control methods are often used to modify SrRuO3. However, these methods are difficult to operate experimentally, have harsh control conditions, and are likely to destroy the crystal structure of the sample, thereby changing the intrinsic properties of the sample. Summary of the invention
[0005] In view of the problems existing in the prior art, the purpose of the present invention is to provide a Co-doped SrRuO3 material with high coercivity and a preparation method thereof. The present invention does not require other operations on the synthesized sample and can be simultaneously regulated during the sample preparation process. The operation is simple, the mixing is uniform, the controllability is strong, and the sample will not be damaged. A Co-doped SrRuO3 material with high coercivity is prepared.
[0006] To achieve the above object, the technical solution adopted by the present invention is:
[0007] A method for preparing a Co-doped SrRuO3 material with high coercivity comprises the following steps:
[0008] Strontium salt, RuO2 and cobalt salt are dispersed in citric acid solution, and concentrated nitric acid is added and mixed evenly to obtain a suspension; preferably, the strontium salt is Sr(NO3)2 or SrCO3; the cobalt salt is Co(NO3)2 or CoCO3; the molar ratio of the strontium salt, cobalt salt and RuO2 is 1:x:(1-x), and the value of x ranges from 0.1 to 0.3.
[0009] The suspension is heated to evaporate the solvent to obtain a solid precursor; citric acid contains carbonyl carboxylic acid, which can act as a chelating agent to generate a metal carboxylate complex with metal cations, and then a dry gel is formed after heating and heat preservation at a certain temperature, achieving uniform mixing at the atomic level, and no intermediate phase is generated during the subsequent sintering process.
[0010] After grinding, the solid precursor is pre-sintered and sintered at high temperature. The sintered product is washed and dried to obtain the target product. Preferably, the pre-sintering temperature is 450-550°C for 6-8 hours; the high-temperature sintering temperature is 900-950°C for 12-15 hours. During the sintering process, a spontaneous combustion reaction of the solid precursor occurs, the decomposition of nitrate accelerates the combustion reaction, and the oxide grains are formed and grown, thereby obtaining the final product.
[0011] In a further solution, the mass fraction of concentrated nitric acid is 64%-80%; the volume ratio of concentrated nitric acid to citric acid solution is 1:6-8. The role of concentrated nitric acid is to act as an oxidant to achieve a low-temperature self-combustion reaction of the solid precursor, which can inhibit grain growth and control particle size.
[0012] The beneficial effects of the present invention are as follows:
[0013] (1) In the preparation process of SrRuO3, the present invention increases the coercivity of the material by doping with Co. The principle is that Co has a smaller radius of ions, and Co doping can induce structural distortion and generate lattice stress, so that Ru 4+ -O-Ru 4+ Ferromagnetism and Co 2+ -O-Ru 5+ / Co 3+ -O-Co 3+ The mutual competition of antiferromagnetism weakens the itinerant characteristics of Ru 4d electrons, resulting in the localization of itinerant electrons and enhancing the coercivity of SrRuO3; in addition, with the increase of Co doping content, the coercivity of the material is further increased, realizing the controllable regulation of the coercivity of doped strontium ruthenate materials.
[0014] (2) The present invention uses citric acid solution as a solvent. Through the chelation effect between citric acid and metal ions, Co ions can be doped into the SrRuO3 lattice at the atomic level, thereby distorting the SrRuO3 structure and reducing the lattice spacing in a certain direction, generating lattice stress. The stress can regulate the orbital occupancy state of electrons and affect the interaction between electron spins, thereby shaping unique magnetic properties.
[0015] (3) Compared with the traditional ball milling mixing and epitaxial growth control method, the present invention realizes control during the material preparation process, is simple to operate, has strong controllability, does not damage the sample, and obtains products with excellent performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] Figure 1 XRD patterns of samples prepared with different doping amounts of Co;
[0017] Figure 2 The magnetic properties test results of samples prepared with different Co doping amounts. DETAILED DESCRIPTION
[0018] The present invention is further described below in conjunction with the embodiments so that those skilled in the art can better understand the present invention and implement it, but the embodiments are not intended to limit the present invention.
[0019] In addition, unless otherwise specified, the preparation processes in the following embodiments are all conventional means in the prior art in the art, and therefore, they are not described in detail; the parts in the following embodiments are all parts by weight.
[0020] Example
[0021] A Co-doped SrRuO3 material with high coercivity and a preparation method thereof, comprising the following steps:
[0022] (1) Sr(NO3)2, Co(NO3)2, and RuO2 were treated according to SrCo x Ru 1-x The solid powder was weighed at a molar ratio of O3, and x was 0, 0.1, 0.2, and 0.3, respectively, and then added to a 0.1 M citric acid solution. 65 wt% concentrated nitric acid was added to the citric acid solution at a volume ratio of 1:7.5 citric acid, and ultrasonicated to obtain a suspension;
[0023] (2) The suspension is placed in an oil bath and heated at 120°C until the solution is completely evaporated to obtain a solid precursor.
[0024] (3) Grind the solid precursor in a mortar for 10 minutes, place the ground sample in a muffle furnace and heat it to 500°C at 5°C / min, and keep it for 6 hours to complete pre-sintering; then increase the temperature to 900°C at 10°C / min and keep it for 12 hours to complete high-temperature sintering; finally, cool it to 500°C at 5°C / min and naturally cool it to room temperature. Wash the obtained sample twice with ethanol and water respectively, and freeze-dry it to obtain the product.
[0025] Figure 1 The XRD patterns of samples prepared with different Co doping amounts are shown in Table 1. Figure 1 It can be seen that with the increase of Co content, the diffraction peak of SrRuO3 moves to a higher angle, the interplanar spacing decreases, and lattice stress is generated.
[0026] Figure 2 The magnetic properties test results of samples prepared with different Co doping amounts are shown in Table 1. Figure 2 It can be seen that with the increase of Co content, the coercivity of SrRuO3 increases.
[0027] It should be noted that, in other embodiments, when the experimental process meets the following conditions, the purpose of the present invention can be achieved:
[0028] The pre-sintering temperature is preferably 450°C-550°C, specifically 450°C, 500°C or 550°C; the pre-sintering time is preferably 6-8h, specifically 6h, 7h or 8h;
[0029] The high temperature sintering temperature is preferably 900-950°C, specifically 900°C, 920°C or 950°C, etc.; the high temperature sintering time is preferably 12-15h, specifically 12h, 13h, 14h or 15h, etc.
[0030] The mass fraction of concentrated nitric acid is preferably 64%-80%, specifically 65%, 70% or 75%; the volume ratio of concentrated nitric acid to citric acid solution is preferably 1:6-8, specifically 1:6, 1:7 or 1:8.
[0031] For the above process parameters, those skilled in the art can make appropriate selections according to actual needs, which can achieve the purpose of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in the field without creative work are within the scope of protection of the present invention.
Claims
1. A Co-doped SrRuO with high coercivity 3 Methods of preparing materials, Features: The following steps are involved: Strontium salt, RuO 2 , cobalt salt is dispersed in citric acid solution, and concentrated nitric acid is added and mixed evenly to obtain a suspension; the mass fraction of the concentrated nitric acid is 64%-80%; the volume ratio of the concentrated nitric acid to the citric acid solution is 1: (6-8); The suspension is heated to evaporate the solvent to obtain a solid precursor; After the solid precursor is ground, it is pre-sintered and sintered at high temperature to obtain the target product; the pre-sintering temperature is 450-550°C and the time is 6-8h; the high-temperature sintering temperature is 900-950°C and the time is 12-15h; The strontium salt, cobalt salt, RuO 2 The molar ratio is 1:x:(1-x), and the value of x ranges from 0.1 to 0.
3.
2. Co-doped SrRuO with high coercivity according to claim 1 3 Methods of preparing materials, Features: The strontium salt is Sr(NO 3 ) 2 or SrCO 3 .
3. Co-doped SrRuO with high coercivity according to claim 1 3 Methods of preparing materials, Features: The cobalt salt is Co(NO 3 ) 2 or CoCO 3 .
4. A Co-doped SrRuO with high coercivity 3 Material, Features: The invention is prepared by the preparation method described in any one of claims 1 to 3.