A high temperature quenched and tempered AOD slag and its preparation method and application, cement filler

By melting and mixing AOD slag with bauxite and cold quenching to generate high-temperature quenched and tempered AOD slag, its glass phase is stimulated to form a gel phase in the cement, which solves the problems of poor cement reinforcement and high Cr element leaching concentration in the existing technology. problem, realizing the preparation of high-performance cement fillers and environmentally friendly resource utilization.

CN116282976BActive Publication Date: 2024-10-22UNIV OF SCI & TECH BEIJING
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211569384.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-08
Publication Date
2024-10-22
Estimated Expiration
2042-12-08

AI Technical Summary

Technical Problem

The existing modified AOD slag has poor cement reinforcement effect and the leaching concentration of Cr element is high, making it difficult to use safely and effectively.

Method used

AOD slag and bauxite are melted and mixed and then quenched to generate high-temperature tempered AOD slag, producing a large amount of glass phase, stimulating the formation of a gel phase in an alkaline cement environment, improving the strength of cement, and controlling Cr through high-pressure water quenching The leaching concentration of the element.

Benefits of technology

It achieves the excellent reinforcing effect of high-temperature conditioned AOD slag on cement. The leaching concentration of Cr element is significantly reduced, reaching high safety standards. It is suitable for cement filler applications, reduces the pollution of solid waste to the environment, and improves resource utilization. .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116282976B_ABST
    Figure CN116282976B_ABST
Patent Text Reader

Abstract

The present invention provides a high temperature quenched and tempered AOD slag and its preparation method and application, cement filler, and relates to the technical field of metallurgical technology. The present invention mixes molten AOD slag with bauxite and then quenches, so that a large amount of glass phase is produced in the high temperature quenched and tempered AOD slag, and the hydration activity, the ability of solidifying chromium and stability are excellent. The leaching concentration of total Cr in the obtained high temperature quenched and tempered AOD slag is ≤0.36mg / L, and the hexavalent chromium leaching concentration is <0.16mg / L, which is far lower than the total Cr and hexavalent chromium leaching standard values ​​in the detoxified chromium slag specified in HJ / T 301-2007. The leaching concentration of Cr element in the high temperature quenched and tempered AOD slag is low, the safety is high, and it has a good application prospect in cement filler. Moreover, the preparation method provided by the present invention has a wide source of raw materials and low price, low production cost, improves the resource utilization rate of AOD slag, reduces the pollution of solid waste to the environment, is safe, and is suitable for industrial production.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of metallurgical technology, and in particular to high-temperature quenched and tempered AOD slag, a preparation method and application thereof, and a cement filler. Background Art

[0002] AOD slag is the remaining refined slag produced by the argon oxygen decarburization refining furnace during the production of stainless steel. It is difficult to use because of its poor activity and the presence of a certain amount of toxic Cr elements that are easily leached. Chinese patent CN114455861A discloses a method for preparing modified AOD slag, comprising the following steps: melting and mixing AOD slag and fly ash, followed by cold quenching, to obtain modified AOD slag, wherein the Cr leaching concentration in the modified AOD slag is 0.042 mg / L, which is much lower than the standard value of 1.5 mg / L Cr leaching in the detoxified chromium slag specified in HJ / T 301-2007. However, the 28-day compressive strength of the cement mortar sample prepared by the modified AOD slag prepared by the above-mentioned prior art is below 54.45 MPa, and the reinforcing effect of the modified AOD slag on cement is not good. Summary of the invention

[0003] In view of this, the object of the present invention is to provide a high-temperature tempered AOD slag and a preparation method and application thereof, and a cement filler. The high-temperature tempered AOD slag prepared by the present invention has excellent reinforcement effect on cement, low leaching concentration of Cr element, and high safety.

[0004] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:

[0005] The present invention provides a method for preparing high-temperature quenched and tempered AOD slag, comprising the following steps:

[0006] Melting and mixing AOD slag and bauxite to obtain molten slag;

[0007] The molten slag is quenched to obtain high temperature tempered AOD slag.

[0008] Preferably, the mass fraction of bauxite in the slag is 15-25wt%.

[0009] Preferably, the water content of the bauxite and AOD slag is independently ≤5wt%.

[0010] Preferably, the temperature of the melt mixing is 1500-1550° C., and the time is 30-60 min.

[0011] Preferably, the cooling rate of the quenching is 800-1000° C. / min.

[0012] Preferably, the cold quenching is high-pressure water quenching, and the pressure of the high-pressure water quenching is 30-50 MPa.

[0013] The present invention provides high-temperature quenched and tempered AOD slag obtained by the preparation method described in the above technical solution, wherein the content of the glass phase in the high-temperature quenched and tempered AOD slag is 97-100%.

[0014] The present invention provides the use of the high-temperature tempered AOD slag described in the above technical solution in cement filler.

[0015] The present invention provides a cement filler, comprising the high-temperature tempered AOD slag described in the above technical solution and cement.

[0016] Preferably, the content of high temperature tempered AOD slag in the cement filler is 20-40wt%.

[0017] The present invention provides a method for preparing high-temperature tempered AOD slag, comprising the following steps: melting and mixing AOD slag and bauxite to obtain slag; quenching the slag to obtain high-temperature tempered AOD slag. The present invention melts and mixes AOD slag with bauxite and then quenches it, so that a large amount of glass phase is generated in the high-temperature tempered AOD slag, which has excellent hydration activity, chromium solidification ability and stability. A large amount of active glass phase is generated in the high-temperature tempered AOD slag, which can be stimulated in the alkaline environment of cement to generate a large amount of gelling phase. Through the hydration and hardening of these gelling phases, excellent strength characteristics are provided for cement materials, and the maximum strength reaches 88.7MPa, meeting the strength requirements of high-performance concrete (40-96MPa). Moreover, the leaching concentration of total Cr in the high-temperature quenched and tempered AOD slag is ≤0.36mg / L, and the leaching concentration of hexavalent chromium is <0.16mg / L, which is far lower than the standard values ​​of 1.5mg / L and 0.5mg / L of total Cr and hexavalent chromium leaching in the detoxified chromium slag specified in HJ / T 301-2007. The leaching concentration of Cr element in the high-temperature quenched and tempered AOD slag is low, the safety is high, and it has a good application prospect in cement fillers. Moreover, the preparation method provided by the present invention has a wide source of raw materials and low prices, low production costs, improves the resource utilization rate of AOD slag, reduces the pollution of solid waste to the environment, has high safety, and provides an effective way for resource-based and harmless coordinated treatment of AOD slag, is suitable for industrial production, and has good environmental and economic benefits.

[0018] The present invention provides high temperature tempered AOD slag obtained by the preparation method described in the above technical solution, wherein the content of glass phase in the high temperature tempered AOD slag is 97-100%. The leaching concentration of total Cr in the high temperature tempered AOD slag provided by the present invention is ≤0.36 mg / L, and the leaching concentration of hexavalent chromium is <0.16 mg / L, which are much lower than the standard values ​​of 1.5 mg / L and 0.5 mg / L for leaching of total Cr and hexavalent chromium in detoxified chromium slag specified in HJ / T 301-2007. The leaching concentration of Cr element in the high temperature tempered AOD slag provided by the present invention is low, the safety is high, and it has a good application prospect in cement fillers.

[0019] The present invention provides a cement filler, comprising the high temperature quenched and tempered AOD slag and cement as described in the above technical solution. In the cement filler provided by the present invention, the activity of the glass phase of the high temperature quenched and tempered AOD slag is stimulated in the alkaline environment of cement, hydrated to generate a gel phase so that the Cr element is stably solidified inside the cement, and the leaching concentrations of total Cr and hexavalent chromium in the cement filler are not higher than 0.09 mg / L and 0.004 mg / L, which are much lower than the standard values ​​of 0.15 mg / L and 0.05 mg / L of total Cr and hexavalent chromium leaching in cement products prepared using chromium-containing slag specified in HJ / T 301-2007, and the safety is high. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 This is the SEM image of the granulated slag prepared in Example 1;

[0021] Figure 2 This is the SEM image of the granulated slag prepared in Comparative Example 2;

[0022] Figure 3 XRD diagrams of the granulated slag prepared in Example 1 and Comparative Examples 1-2;

[0023] Figure 4 The 28-day compressive strength test results of cement mortar samples made of cement fillers prepared in Examples 1 to 3 and Comparative Examples 1 to 2 are shown;

[0024] Figure 5 This is a graph showing the test results of Cr element leaching concentration in high temperature tempered AOD slag prepared in Examples 1 to 3 and Comparative Examples 1 to 2;

[0025] Figure 6 This is the test result diagram of Cr element leaching concentration in the cement mortar sample prepared in Test Example 2. DETAILED DESCRIPTION

[0026] The present invention provides a method for preparing high-temperature quenched and tempered AOD slag, comprising the following steps:

[0027] Melting and mixing AOD slag and bauxite to obtain molten slag;

[0028] The molten slag is quenched to obtain high temperature tempered AOD slag.

[0029] In the present invention, unless otherwise specified, all raw material components are commercially available products well known to those skilled in the art.

[0030] The invention melts and mixes AOD slag and bauxite to obtain molten slag.

[0031] The present invention does not specifically limit the source of the AOD slag, and the AOD slag well known to those skilled in the art can be used; in a specific embodiment of the present invention, the AOD slag is preferably a refined slag produced by argon oxygen decarburization furnace refining in a stainless steel production enterprise; the chemical composition of the AOD slag preferably includes: CaO 55-60wt%, more preferably 56-59wt%, and more preferably 57-58wt%; SiO2 25-30wt%, more preferably 26-29wt%, and more preferably 27-28wt%; Cr2O3 1-3wt%, more preferably 1.5-2.5wt%, and more preferably 2-2.5wt%; MgO 2-5wt%, more preferably 2.5-4.5wt%, and more preferably 3-4wt%. In the present invention, the water content of the AOD slag is preferably ≤5wt%, more preferably 0.5-5wt%, and more preferably 1-2wt%.

[0032] The present invention has no special limitation on the source of the bauxite, and bauxite well known to those skilled in the art can be used; in a specific embodiment of the present invention, the bauxite is preferably bauxite used for aluminum smelting or preparing refractory materials; the chemical composition of the bauxite preferably includes: Al2O375-80wt%, more preferably 77-80wt%, and further preferably 78-80wt%; SiO28-11wt%, more preferably 9-11wt%, and further preferably 10-11wt%; Ti2O31-4wt%, more preferably 2-4wt%, and further preferably 3-4wt%. In the present invention, the water content of the bauxite is preferably ≤5wt%, more preferably 0.5-5wt%, and further preferably 1-2wt%; the present invention controls the water content in the bauxite within the above range, and can achieve the safe production of high-temperature quenched and tempered AOD slag.

[0033] In the present invention, the temperature of the melt mixing is preferably 1500-1550°C, more preferably 1520-1550°C, and further preferably 1540-1550°C; the heating rate from room temperature to the temperature of the melt mixing is preferably 10-15°C / min, more preferably 11-14°C / min, and further preferably 12-13°C / min; starting from the temperature rising to the temperature of the melt mixing, the holding time of the melt mixing is preferably 30-60min, more preferably 35-55min, and further preferably 40-50min; the present invention performs melt mixing within the above temperature range, and the AOD slag and bauxite have good fluidity, and can achieve full and uniform mixing of the two, thereby improving the strength of the high-temperature quenched and tempered AOD slag. In the present invention, the melt mixing is preferably: pre-mixing the AOD slag and bauxite and then melt mixing, or directly melt mixing the molten AOD slag and bauxite. The present invention has no special limitation on the pre-mixing, and the raw materials can be mixed evenly. In a specific embodiment of the present invention, the melt mixing is preferably carried out in a vertical resistance furnace. In the present invention, when the molten AOD slag and bauxite are directly melted and mixed, the bauxite is preferably added to the molten AOD slag in batches for mixing; the number of times the bauxite is added is preferably 3 to 5 times, more preferably 4 times.

[0034] In the present invention, the mass fraction of bauxite in the slag is preferably 12-15wt%, more preferably 13-15wt%, and further preferably 14-15wt%. In the present invention, the amount of bauxite doped is small, which can greatly improve the resource utilization rate of AOD slag, reduce the pollution of solid waste to the environment, and has high safety. It provides an effective way for resource-based and harmless coordinated treatment of AOD slag, is suitable for industrial production, and has good environmental and economic benefits.

[0035] After obtaining the slag, the present invention quenches the slag to obtain high-temperature tempered AOD slag.

[0036] In the present invention, the cooling rate of the cold quenching is preferably 800-1000°C / min, more preferably 850-950°C / min, and further preferably 900°C / min; in the present invention, the cold quenching is preferably high-pressure water quenching, and the water pressure of the high-pressure water quenching is preferably 30-50MPa, more preferably 35-45MPa, and further preferably 40MPa.

[0037] After the cold quenching, the present invention preferably further comprises crushing the granulated slag obtained by the cold quenching to obtain high temperature tempered AOD slag. The present invention has no special limitation on the crushing, and the crushing can be performed to a particle size of ≤0.1 mm using a crushing method well known to those skilled in the art, such as grinding.

[0038] The present invention provides a high temperature tempered AOD slag obtained by the preparation method described in the above technical solution. In the present invention, the content of the glass phase in the high temperature tempered AOD slag is 97-100%, preferably 98-100%. In the present invention, the particle size of the high temperature tempered AOD slag is preferably ≤0.1mm. In the present invention, the specific surface area of ​​the high temperature tempered AOD slag is preferably ≥500m 2 / kg, more preferably 500 to 600 m 2 / kg.

[0039] The present invention provides the application of the high temperature tempered AOD slag described in the above technical solution in cement fillers. The leaching concentration of total Cr in the high temperature tempered AOD slag provided by the present invention is ≤0.36 mg / L, and the leaching concentration of hexavalent chromium is <0.16 mg / L. The leaching concentration of Cr element in the high temperature tempered AOD slag provided by the present invention is low, the safety is high, and it has a good application prospect in cement fillers.

[0040] The present invention provides a cement filler, comprising the high temperature tempered AOD slag and cement described in the above technical solution. In the present invention, the content of the high temperature tempered AOD slag in the cement filler is preferably 20-40wt%, more preferably 25-35wt%, and further preferably 30wt%. In the present invention, the cement preferably comprises silicate cement.

[0041] The technical solutions in the present invention will be described clearly and completely below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only a part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0042] Example 1

[0043] (1) High temperature tempering of AOD slag

[0044] 85 g of AOD slag and 15 g of bauxite were mixed evenly and placed in a corundum crucible. The corundum crucible was placed in a vertical resistance furnace, and the temperature was increased to 1550° C. at a heating rate of 10° C. / min. The mixture was kept warm for 60 minutes to obtain slag.

[0045] The corundum crucible was removed from the vertical resistance furnace and subjected to high pressure water quenching at a cooling rate of 800°C / min. The obtained granulated slag was ground to obtain high temperature quenched and tempered AOD slag with a particle size of 0.08 mm (specific surface area of ​​542 m 2 / kg), wherein the water pressure of high-pressure water quenching is 30MPa.

[0046] (2) Cement filler

[0047] The high temperature tempered AOD slag and the silicate cement clinker are mixed in a mass ratio of 3:7 to obtain a cement filler.

[0048] Example 2

[0049] High temperature tempered AOD slag and cement filler were prepared according to the method of Example 1, except that the amount of AOD slag used was 80 g and the amount of bauxite used was 20 g.

[0050] Example 3

[0051] High temperature tempered AOD slag and cement filler were prepared according to the method of Example 1, except that the amount of AOD slag used was 75 g and the amount of bauxite used was 25 g.

[0052] Comparative Example 1

[0053] High temperature tempered AOD slag and cement filler were prepared according to the method of Example 1, except that the amount of AOD slag used was 100 g, and no bauxite was added.

[0054] Comparative Example 2

[0055] High temperature tempered AOD slag and cement filler were prepared according to the method of Example 1, except that the amount of AOD slag used was 90 g and the amount of bauxite used was 10 g.

[0056] Test Example 1

[0057] Figure 1 This is the SEM image of the granulated slag prepared in Example 1. Figure 2 The SEM image of the granulated slag prepared in Comparative Example 2 is Figures 1-2 It can be seen that the granulated slag prepared in Comparative Example 2 has crystalline phase precipitation, while the granulated slag prepared in Example 1 is all glassy.

[0058] Figure 3 The XRD patterns of the granulated slag prepared in Example 1 and Comparative Examples 1-2 are shown in FIG. Figure 3 It can be seen that the main phase of high-temperature tempered AOD slag with a bauxite addition of 10wt% is Ca2Al2SiO7, and the main phase of high-temperature tempered AOD slag with a bauxite addition of 15wt% is pure glass phase. The glass phase has high potential activity. After being mixed with silicate cement clinker to prepare stainless steel slag cement, hydration hardening gelation reaction can occur; while after melting and quenching of AOD slag without bauxite, the main crystal phase includes γ-Ca2SiO4, MgO and CaF2, and no glass phase appears.

[0059] Test Example 2

[0060] The cement fillers prepared in Examples 1 to 3 and Comparative Examples 1 to 2 were respectively mixed with standard sand in a mass ratio of 1:3 and a water-cement ratio of 0.5, and placed in a 40×40×160 mm steel mold for 24 h, demolded, and then taken out after curing in a standard curing box for 28 days to obtain cement mortar samples.

[0061] (1) 28-day compressive strength test of cement mortar specimens.

[0062] Figure 4 The 28-day compressive strength test results of cement mortar samples made of cement fillers prepared in Examples 1 to 3 and Comparative Examples 1 to 2 are shown in FIG. Figure 4 It can be seen that the compressive strength of the cement filler prepared by using the high-temperature tempered AOD slag without adding bauxite reaches 66.56 MPa; the compressive strength of the cement filler prepared by using the high-temperature tempered AOD slag prepared by the embodiment of the present invention is higher than 88.7 MPa.

[0063] (2) Total Cr and hexavalent chromium leaching concentrations in high temperature quenched and tempered AOD slag and cement mortar samples

[0064] The total Cr and hexavalent chromium leaching concentrations in the high temperature tempered AOD slag prepared in Examples 1 to 3 and Comparative Examples 1 to 2 were tested according to "Solid Waste Leaching Toxicity Leaching Method Sulfuric Acid and Nitric Acid Method" (HJ / T 299-2010).

[0065] According to the Technical Specification for Environmental Protection of Chromium Slag Pollution Control (HJ / T 301-2007), the leaching concentration of Cr element in cement mortar samples prepared from the high-temperature tempered AOD slag obtained in Examples 1 to 3 and Comparative Examples 1 to 2 was tested.

[0066] Figure 5 The graph is a test result of Cr element leaching concentration in high temperature quenched and tempered AOD slag prepared in Examples 1 to 3 and Comparative Examples 1 to 2. Figure 5 It can be seen that the Cr leaching concentration in the high-temperature tempered AOD slag without adding bauxite is 1.7 mg / L, and the hexavalent Cr leaching concentration is 0.1 mg / L, while the Cr leaching concentration in the high-temperature tempered AOD slag prepared by Examples 1 to 3 of the present invention is 0.27-0.36 mg / L, and the hexavalent Cr leaching concentration is 0.12-0.16 mg / L, which are much lower than the standard value of 1.5 mg / L for total Cr leaching and 0.5 mg / L for hexavalent Cr leaching in the detoxified chromium slag specified in HJ / T 301-2007.

[0067] Figure 6The graph shows the test results of Cr element leaching concentration in cement mortar samples made of cement fillers prepared in Examples 1 to 3 and Comparative Examples 1 to 2. The total Cr leaching concentration in the cement mortar sample prepared using high temperature quenched and tempered AOD slag without adding bauxite is 0.125 mg / L, and the hexavalent Cr leaching concentration is 0.001 mg / L, while the total Cr leaching concentration in the cement mortar sample prepared using high temperature quenched and tempered AOD slag prepared in Examples 1 to 3 of the present invention is 0.05-0.09 mg / L, and the hexavalent Cr leaching concentration is 0.002-0.004 mg / L, which is much lower than the standard value of 0.15 mg / L for total Cr leaching and 0.05 mg / L for hexavalent Cr leaching in cement products prepared using chromium-containing slag as specified in HJ / T 301-2007.

[0068] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A method for preparing high temperature tempered AOD slag, The following steps are involved: The AOD slag and bauxite are melted and mixed to obtain slag; the mass fraction of bauxite in the slag is 15-25wt%; The slag is cold quenched to obtain high-temperature tempered AOD slag; the cooling rate of the cold quenching is 800-1000°C / min; the cold quenching is high-pressure water quenching, and the pressure of the high-pressure water quenching is 30-50MPa.

2. The preparation method according to claim 1, It is characterized in that The water content of the bauxite and the AOD slag is independently ≤5wt%.

3. The preparation method according to claim 1, It is characterized in that The temperature of the melt mixing is 1500-1550° C. and the time is 30-60 min.

4. The high temperature tempered AOD slag obtained by the preparation method according to any one of claims 1 to 3, wherein the content of the glass phase in the high temperature tempered AOD slag is 97 to 100%.

5. Use of the high temperature tempered AOD slag according to claim 4 in cement filler.

6. A cement filler comprising the high temperature tempered AOD slag according to claim 4 and cement.

7. The cement filler according to claim 6, It is characterized in that The content of high temperature tempered AOD slag in the cement filler is 20-40wt%.