Antistatic thermal expansion microsphere, polyacrylate foam and preparation method and application thereof
By using thermally expanded microspheres with silver-plated surface and ester-based functionalization in polyacrylate foam, the conductive path and compatible interface are formed, and the problem of electrostatic charge accumulation of polyacrylate foam is solved, which significantly improves the anti-static properties and stability.
Patent Information
- Application Number
- CN202310388056.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-12
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2043-04-12
AI Technical Summary
The existing polyacrylate foam dissipates slowly when the electrostatic charge accumulates, resulting in electrostatic charge accumulation, affecting the stability of the material and interference of electronic signals.
The thermally expanded microspheres with silver plating and ester group functionalization were used to form a thermally expanded microspheres of ammonia oxime by hydroxylamine functionalization treatment, and the silver plating was deposited with silver nitrate and glucose, and then functionalized with methyl thioglycolate. Antistatic thermal expansion microspheres were prepared and combined in polyacrylate foam to form conductive paths and compatible interfaces to improve antistatic properties.
The leakage of charge through the conductive pathway significantly improves the antistatic properties, and the dispersion is improved through ester-based functionalization, thereby enhancing the stability and performance of the antistatic polyacrylate foam.
Smart Images

Figure BDA0004174799550000041 
Figure HDA0004174799560000011
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of polymer materials, and in particular to an antistatic thermal expansion microsphere, polyacrylate foam, and a preparation method and application thereof. Background Art
[0002] In modern industrial production and daily life, the accumulation of static charges often causes significant losses and disasters. When materials come into contact or separate from each other, charges are generated and dissipated. This is usually a dynamic equilibrium process. However, when the charge accumulation time is long enough, the charge generation is faster than the dissipation, and the balance is broken. A large amount of static charge that cannot be dissipated will accumulate on the surface of the material, forming an electric field and generating a potential difference. When the potential difference is large enough, the electric field generated by the potential difference will break through the inside of the material or the air to discharge. The discharge phenomenon is usually accompanied by material damage or interference with electronic signals and circuit boards.
[0003] Take the OLED screen as an example. In order to protect the OLED screen from the impact of falling or collision, which may cause product failure, a layer of buffer foam is added between the back of the OLED screen and the shell. Polyacrylate is one of the commonly used foam materials under the screen of OLED screens, but it dissipates charge slowly and has poor antistatic effect, which can easily cause the accumulation of static charge, leading to material damage or interference with electronic signals and circuit boards. Therefore, it is of great significance to develop a polyacrylate foam with antistatic function. Summary of the invention
[0004] The technical problem to be solved by the present invention is to provide an antistatic heat-expandable microsphere and polyacrylate foam, so as to solve the problem that the polyacrylate foam in the prior art cannot meet the antistatic requirement.
[0005] In order to solve the above technical problems, the technical solution of the present invention is as follows:
[0006] The invention discloses an antistatic heat-expandable microsphere, which is a heat-expandable microsphere with silver-plated surface and ester group functionalized.
[0007] Preferably, the antistatic heat-expandable microspheres are silver-plated by surface hydroxylamine functionalization.
[0008] The present invention also provides a method for preparing antistatic heat-expandable microspheres, comprising the following steps:
[0009] (1) mixing hydroxylamine with heat-expandable microspheres to obtain ammonia oxime heat-expandable microspheres;
[0010] (2) mixing the ammoxime heat-expandable microspheres obtained in step (1) with silver nitrate, ammonia water, and glucose to obtain heat-expandable microspheres with silver-plated surfaces;
[0011] (3) mixing the silver-plated heat-expandable microspheres obtained in step (2) with methyl thioglycolate to obtain antistatic heat-expandable microspheres.
[0012] Preferably, in step (1), the weight ratio of the heat-expandable microspheres to hydroxylamine is 1:(4-8);
[0013] More preferably, in step (1), the reaction temperature is 60-90° C. and the reaction time is 10-30 min.
[0014] Preferably, in step (2), the weight ratio of the amidoxime heat-expandable microspheres to silver nitrate is 1:(1-15);
[0015] Further preferably, in step (2), the molar ratio of silver nitrate, ammonia water and glucose is 1:(2-4):(3-6);
[0016] More preferably, in step (2), the reaction time is 4-8 hours.
[0017] Preferably, in step (3), the weight ratio of the silver-plated heat-expandable microspheres to methyl thioglycolate is 1:(1-3);
[0018] More preferably, in step (3), the reaction time is 6-10 h.
[0019] The present invention also provides an antistatic polyacrylate foam, comprising the antistatic thermal expansion microspheres.
[0020] Preferably, the antistatic polyacrylate foam further comprises an acrylate monomer, an initiator, and a cross-linking agent.
[0021] Preferably, the antistatic polyacrylate foam comprises the following raw materials in parts by weight: 0.1-0.3 parts of initiator, 1-2 parts of cross-linking agent, and 5-10 parts of antistatic heat-expandable microspheres per 100 parts of acrylate monomer.
[0022] The present invention also provides application of the antistatic heat-expandable microspheres in polyacrylate foam.
[0023] The above solution of the present invention includes at least the following beneficial effects:
[0024] (1) The antistatic heat-expandable microspheres of the present invention are heat-expandable microspheres with silver-plated surfaces and ester-functionalized. Since silver itself has excellent electrical conductivity, when the silver-plated heat-expandable microspheres are added to polyacrylate foam, a conductive path is formed in the matrix, and charges leak through the conductive path, thereby achieving an antistatic effect; ester functionalization is performed on the silver-plated heat-expandable microspheres by grafting ester groups. Since the ester groups have similar polarities to the target matrix, after the heat-expandable microspheres with silver-plated surfaces and ester-functionalized are added to the polyacrylate foam, a compatible interface can be formed, which improves their dispersibility in the polyacrylate foam, thereby making the antistatic polyacrylate foam have good antistatic properties.
[0025] (2) The antistatic heat-expandable microspheres of the present invention are silver-plated by surface hydroxylamine functionalization. The surface of the heat-expandable microspheres contains cyano groups. Through the surface hydroxylamine functionalization treatment, hydroxylamine and cyano groups interact to form amidoxime (-C(NH2)=N-O), so that polar hydroxyl groups and amino groups with complexing properties for silver are generated on the surface of the heat-expandable microspheres. The polar hydroxyl groups can serve as catalytic centers during the silver plating process to deposit silver ions on the surface of the microspheres; the amino groups with complexing properties for silver can make the silver ions firmly bond to the surface of the microspheres, obtain a coating that is not easy to peel off, and enhance the stability of the silver-plated microspheres.
[0026] (3) The preparation method of the antistatic heat-expandable microspheres of the present invention comprises the following steps: mixing hydroxylamine with heat-expandable microspheres to obtain amidoxime heat-expandable microspheres; mixing the amidoxime heat-expandable microspheres with silver nitrate, ammonia water and glucose to obtain heat-expandable microspheres with silver-plated surfaces; mixing the heat-expandable microspheres with silver-plated surfaces with methyl thioglycolate to obtain antistatic heat-expandable microspheres. After the hydroxylamine is mixed with the heat-expandable microspheres, the hydroxylamine reacts with the cyano group on the surface of the heat-expandable microspheres to form ammonia (-C(NH2)=N-O) on the surface of the heat-expandable microspheres, and the ammonia heat-expandable microspheres are obtained, and the surface of the ammonia heat-expandable microspheres has polar hydroxyl groups and amino groups with complexing properties for silver; after the ammonia heat-expandable microspheres are mixed with silver nitrate, ammonia water, and glucose, the polar hydroxyl groups can be used as catalytic centers to deposit silver ions in the silver nitrate on the surface of the microspheres, and the amino groups with complexing properties for silver firmly bind the silver ions on the surface of the ammonia heat-expandable microspheres, and the glucose is used as a reducing agent to reduce the silver ions to silver elemental substance, and the heat-expandable microspheres with silver-plated surfaces are obtained; the heat-expandable microspheres with silver-plated surfaces are mixed with methyl thioglycolate, and ester groups are functionalized by grafting ester groups to obtain the antistatic heat-expandable microspheres. The preparation process is simple, the reaction conditions are mild, and it is suitable for large-scale production.
[0027] (4) The antistatic polyacrylate foam of the present invention is blended with the antistatic heat-expandable microspheres. After the silver coating on the surface of the antistatic heat-expandable microspheres diffuses in the polyacrylate foam, a conductive path is formed, so that charges can leak through the conductive path, thereby making the antistatic polyacrylate foam have good antistatic properties; ester functionalization can increase the dispersibility of the antistatic heat-expandable microspheres in the antistatic polyacrylate foam, thereby improving its antistatic properties. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 This is the synthesis route of the antistatic heat-expandable microspheres of the present invention. DETAILED DESCRIPTION
[0029] If the specific conditions are not specified in the embodiments of the present invention, the conventional conditions or the conditions recommended by the manufacturer are used. If the manufacturer of the reagents or instruments is not specified, they are all conventional products that can be obtained commercially. Only some of the reagents used in the embodiments of the present invention are provided below. Raw materials of different manufacturers and models do not affect the implementation of the technical solution of the present invention and the realization of the technical effects.
[0030]
[0031] Example 1
[0032] The antistatic heat-expandable microspheres of this embodiment are heat-expandable microspheres with silver-plated and ester-functionalized surfaces. The synthesis route of the antistatic heat-expandable microspheres is as follows: Figure 1 shown.
[0033] The method for preparing the antistatic heat-expandable microspheres described in this embodiment comprises the following steps:
[0034] (1) taking hydroxylamine and heat-expandable microspheres, preparing the hydroxylamine into a hydroxylamine aqueous solution with a concentration of 1 mol / L, dispersing the heat-expandable microspheres in the hydroxylamine aqueous solution, stirring and reacting at 80° C. for 15 min, to obtain ammoxime heat-expandable microspheres; the weight ratio of the heat-expandable microspheres to the hydroxylamine is 1:5;
[0035] (2) dispersing the ammonia oxime heat-expandable microspheres obtained in step (1) with silver nitrate, ammonia water, and glucose in deionized water, and reacting them at room temperature for 8 hours to obtain heat-expandable microspheres with silver-plated surfaces; the weight ratio of the ammonia oxime heat-expandable microspheres to silver nitrate is 1:3, and the molar ratio of the silver nitrate, ammonia water, and glucose is 1:3:5;
[0036] (3) mixing the silver-plated heat-expandable microspheres obtained in step (2) with methyl thioglycolate, dispersing the silver-plated heat-expandable microspheres and methyl thioglycolate in deionized water under nitrogen protection, stirring and reacting at room temperature for 8 hours to obtain antistatic heat-expandable microspheres. The weight ratio of the silver-plated heat-expandable microspheres to methyl thioglycolate is 1:2.
[0037] The antistatic polyacrylate foam of this embodiment includes the following raw materials in parts by weight: 100 parts of acrylate monomer, 0.3 parts of initiator, 1 part of cross-linking agent, and 5 parts of antistatic heat-expandable microspheres. The acrylate monomer is a mixture of butyl acrylate and isooctyl acrylate in a weight ratio of 65:35; the initiator is azobisisobutyronitrile; and the cross-linking agent is ethylene glycol dimethacrylate.
[0038] The preparation method of the antistatic polyacrylate foam described in this embodiment is as follows:
[0039] Acrylate monomer, initiator, crosslinking agent and antistatic heat-expandable microspheres are taken in parts by weight and mixed evenly. The mixture is first subjected to a prepolymerization reaction at 70°C for 1 hour, and then the obtained prepolymer is coated on a release film and placed in a blast oven at 80°C for polymerization reaction to expand the heat-expandable microspheres to obtain an antistatic polyacrylate foam.
[0040] Example 2
[0041] The antistatic heat-expandable microspheres of this embodiment are heat-expandable microspheres with silver-plated and ester-functionalized surfaces. The synthesis route of the antistatic heat-expandable microspheres is as follows: Figure 1 shown.
[0042] The method for preparing the antistatic heat-expandable microspheres described in this embodiment comprises the following steps:
[0043] (1) taking hydroxylamine and heat-expandable microspheres, preparing the hydroxylamine into a hydroxylamine aqueous solution with a concentration of 1 mol / L, dispersing the heat-expandable microspheres in the hydroxylamine aqueous solution, stirring and reacting at 60° C. for 10 min, to obtain ammoxime heat-expandable microspheres; the weight ratio of the heat-expandable microspheres to the hydroxylamine is 1:4;
[0044] (2) dispersing the ammonia oxime heat-expandable microspheres obtained in step (1) with silver nitrate, ammonia water, and glucose in deionized water, and reacting them at room temperature for 5 hours to obtain heat-expandable microspheres with silver-plated surfaces; the weight ratio of the ammonia oxime heat-expandable microspheres to silver nitrate is 1:1, and the molar ratio of the silver nitrate, ammonia water, and glucose is 1:2:6;
[0045] (3) mixing the silver-plated heat-expandable microspheres obtained in step (2) with methyl thioglycolate, dispersing the silver-plated heat-expandable microspheres and methyl thioglycolate in deionized water under nitrogen protection, stirring and reacting at room temperature for 6 hours to obtain antistatic heat-expandable microspheres. The weight ratio of the silver-plated heat-expandable microspheres to the methyl thioglycolate is 1:1.
[0046] The raw materials and preparation method of the antistatic polyacrylate foam of this embodiment are the same as those of Example 1.
[0047] Example 3
[0048] The antistatic heat-expandable microspheres of this embodiment are heat-expandable microspheres with silver-plated and ester-functionalized surfaces. The synthesis route of the antistatic heat-expandable microspheres is as follows: Figure 1 shown.
[0049] The method for preparing the antistatic heat-expandable microspheres described in this embodiment comprises the following steps:
[0050] (1) taking hydroxylamine and heat-expandable microspheres, preparing the hydroxylamine into a hydroxylamine aqueous solution with a concentration of 1 mol / L, dispersing the heat-expandable microspheres in the hydroxylamine aqueous solution, stirring and reacting at 90° C. for 30 min, to obtain ammoxime heat-expandable microspheres; the weight ratio of the heat-expandable microspheres to the hydroxylamine is 1:8;
[0051] (2) dispersing the ammonia oxime heat-expandable microspheres obtained in step (1) with silver nitrate, ammonia water, and glucose in deionized water, and reacting them at room temperature for 4 hours to obtain heat-expandable microspheres with silver-plated surfaces; the weight ratio of the ammonia oxime heat-expandable microspheres to silver nitrate is 1:15, and the molar ratio of the silver nitrate, ammonia water, and glucose is 1:4:3;
[0052] (3) mixing the silver-plated heat-expandable microspheres obtained in step (2) with methyl thioglycolate, dispersing the silver-plated heat-expandable microspheres and methyl thioglycolate in deionized water under nitrogen protection, stirring and reacting at room temperature for 10 hours to obtain antistatic heat-expandable microspheres. The weight ratio of the silver-plated heat-expandable microspheres to methyl thioglycolate is 1:3.
[0053] The raw materials and preparation method of the antistatic polyacrylate foam of this embodiment are the same as those of Example 1.
[0054] Example 4
[0055] The antistatic heat-expandable microspheres of this embodiment are heat-expandable microspheres with silver-plated and ester-functionalized surfaces. The synthesis route of the antistatic heat-expandable microspheres is as follows: Figure 1 shown.
[0056] The method for preparing the antistatic heat-expandable microspheres described in this embodiment comprises the following steps:
[0057] (1) taking hydroxylamine and heat-expandable microspheres, preparing the hydroxylamine into a hydroxylamine aqueous solution with a concentration of 1 mol / L, dispersing the heat-expandable microspheres in the hydroxylamine aqueous solution, stirring and reacting at 75° C. for 15 min, to obtain ammoxime heat-expandable microspheres; the weight ratio of the heat-expandable microspheres to the hydroxylamine is 1:6;
[0058] (2) dispersing the ammonia oxime heat-expandable microspheres obtained in step (1) with silver nitrate, ammonia water, and glucose in deionized water, and reacting them at room temperature for 8 hours to obtain heat-expandable microspheres with silver-plated surfaces; the weight ratio of the ammonia oxime heat-expandable microspheres to silver nitrate is 1:6, and the molar ratio of the silver nitrate, ammonia water, and glucose is 1:4:6;
[0059] (3) mixing the silver-plated heat-expandable microspheres obtained in step (2) with methyl thioglycolate, dispersing the silver-plated heat-expandable microspheres and methyl thioglycolate in deionized water under nitrogen protection, stirring and reacting at room temperature for 8 hours to obtain antistatic heat-expandable microspheres. The weight ratio of the silver-plated heat-expandable microspheres to methyl thioglycolate is 1:2.
[0060] The raw materials and preparation method of the antistatic polyacrylate foam of this embodiment are the same as those of Example 1.
[0061] Example 5
[0062] The antistatic heat-expandable microspheres of this embodiment are heat-expandable microspheres with silver-plated and ester-functionalized surfaces. The synthesis route of the antistatic heat-expandable microspheres is as follows: Figure 1 shown.
[0063] The preparation method of the antistatic heat-expandable microspheres described in this embodiment is the same as that in embodiment 1. The only difference is that the weight ratio of the ammoxime heat-expandable microspheres to silver nitrate is 1:1.
[0064] The raw materials and preparation method of the antistatic polyacrylate foam of this embodiment are the same as those of Example 1.
[0065] Example 6
[0066] The antistatic heat-expandable microspheres of this embodiment are heat-expandable microspheres with silver-plated and ester-functionalized surfaces. The synthesis route of the antistatic heat-expandable microspheres is as follows: Figure 1 shown.
[0067] The preparation method of the antistatic heat-expandable microspheres described in this embodiment is the same as that in embodiment 1. The only difference is that the weight ratio of the ammoxime heat-expandable microspheres to silver nitrate is 1:2.
[0068] The raw materials and preparation method of the antistatic polyacrylate foam of this embodiment are the same as those of Example 1.
[0069] Example 7
[0070] The antistatic heat-expandable microspheres of this embodiment are heat-expandable microspheres with silver-plated and ester-functionalized surfaces. The synthesis route of the antistatic heat-expandable microspheres is as follows: Figure 1 shown.
[0071] The preparation method of the antistatic heat-expandable microspheres described in this embodiment is the same as that in embodiment 1. The only difference is that the weight ratio of the ammoxime heat-expandable microspheres to silver nitrate is 1:5.
[0072] The raw materials and preparation method of the antistatic polyacrylate foam of this embodiment are the same as those of Example 1.
[0073] Comparative Example 1
[0074] The raw materials and preparation method of the antistatic polyacrylate foam of this comparative example are the same as those of Example 1. The only difference is that the antistatic heat-expandable microspheres are replaced by heat-expandable microspheres.
[0075] Comparative Example 2
[0076] The raw materials and preparation method of the antistatic polyacrylate foam of this comparative example are the same as those of Example 1. The only difference is that the antistatic heat-expandable microspheres are replaced by heat-expandable microspheres that are only silver-plated and not ester-functionalized.
[0077] Effect comparison ratio
[0078] In order to verify the technical effect of the antistatic polyacrylate foam described in the present invention, the following test was carried out:
[0079] Take the antistatic polyacrylate foam prepared in Examples 1-7 and the polyacrylate foam prepared in Comparative Examples 1-2, let them stand for 24 hours, and then measure their volume resistivity. Cut a 200mm*100mm*0.2mm test sample, use an ohmmeter with a positive and negative test pen distance of 1 cm to measure its resistance, read the ohmmeter display of a relatively stable value, change the measurement position, repeat several times, and take the average value, which is the resistance value R of the sample. V The measured resistance value R V , electrode area S, sample thickness h, according to the formula The volume resistivity ρ of the sample is calculated V .
[0080] After experimentation, the results are as follows:
[0081] Serial number Volume resistivity (Ω﹒m) Example 1 <![CDATA[7.7×10 7 ]]> Example 2 <![CDATA[1.2×10 9 ]]> Example 3 <![CDATA[1.2×10 8 ]]> Example 4 <![CDATA[8.3×10 8 ]]> Example 5 <![CDATA[5.6×10 10 ]]> Example 6 <![CDATA[1.2×10 9 ]]> Example 7 <![CDATA[2.6×10 7 ]]> Comparative Example 1 <![CDATA[3.9×10 13 ]]> Comparative Example 2 <![CDATA[1.6×10 10 ]]>
[0082] According to the comparison between Examples 1-7 and Comparative Example 1, the antistatic polyacrylate foam blended with the antistatic heat-expandable microspheres has a lower resistivity, which indicates that the silver plating on the surface of the antistatic heat-expandable microspheres diffuses in the polyacrylate foam to form a conductive path, so that the charge can leak through the conductive path, thereby making the antistatic polyacrylate foam have good antistatic properties.
[0083] According to the comparison between Examples 1-7 and Comparative Example 2, the antistatic polyacrylate foam prepared from the heat-expandable microspheres with silver-plated surfaces and ester-functionalized heat-expandable microspheres has a lower resistivity than the heat-expandable microspheres with silver-plated surfaces and not ester-functionalized heat-expandable microspheres, indicating that ester functionalization can increase the dispersibility of the antistatic heat-expandable microspheres in the antistatic polyacrylate foam and improve its antistatic performance.
[0084] According to the comparison between Example 1 and Examples 5-7, the antistatic performance of the antistatic polyacrylate foam increases with the increase of the amount of silver nitrate. When the amount of silver nitrate reaches a certain level, the antistatic performance of the antistatic polyacrylate foam is limited. When the mass ratio of the heat-expandable microspheres to the silver nitrate is 1:3, the optimal antistatic performance can be obtained while controlling the cost.
[0085] It is known from common technical knowledge that the present invention can be implemented by other embodiments that do not deviate from its spirit or essential features. Therefore, the above disclosed embodiments are only illustrative in all respects and are not exclusive. All changes within the scope of the present invention or within the scope equivalent to the present invention are included in the present invention.
Claims
1. A method for preparing antistatic heat-expandable microspheres, characterized in that: The antistatic heat-expandable microspheres are heat-expandable microspheres with silver-plated and ester-functionalized surfaces, and the surfaces of the heat-expandable microspheres contain cyano groups; The antistatic heat-expandable microspheres are prepared by the following steps: (1) mixing hydroxylamine with heat-expandable microspheres to obtain ammonia oxime heat-expandable microspheres; (2) mixing the ammoxime heat-expandable microspheres obtained in step (1) with silver nitrate, ammonia water, and glucose to obtain heat-expandable microspheres with silver-plated surfaces; (3) mixing the silver-plated heat-expandable microspheres obtained in step (2) with methyl thioglycolate to obtain antistatic heat-expandable microspheres.
2. The method for preparing antistatic heat-expandable microspheres according to claim 1, characterized in that: In step (1), the weight ratio of the heat-expandable microspheres to hydroxylamine is 1:(4-8); Optionally, in step (1), the reaction temperature is 60-90° C. and the reaction time is 10-30 min.
3. The method for preparing antistatic heat-expandable microspheres according to claim 1, characterized in that: In step (2), the weight ratio of the amidoxime heat-expandable microspheres to silver nitrate is 1:(1-15); Optionally, in step (2), the molar ratio of silver nitrate, aqueous ammonia and glucose is 1:(2-4):(3-6); Optionally, in step (2), the reaction time is 4-8 hours.
4. The method for preparing antistatic heat-expandable microspheres according to claim 1, characterized in that: In step (3), the weight ratio of the silver-plated heat-expandable microspheres to methyl thioglycolate is 1:(1-3); Optionally, in step (3), the reaction time is 6-10 h. 5.An antistatic heat-expandable microsphere, characterized in that: The antistatic heat-expandable microspheres are prepared by the method according to any one of claims 1 to 4.
6. An antistatic polyacrylate foam, characterized in that: The invention relates to antistatic heat-expandable microspheres prepared by the method described in any one of claims 1 to 4.
7. The antistatic polyacrylate foam according to claim 6, characterized in that: It also includes acrylate monomers, initiators, and crosslinking agents.
8. The antistatic polyacrylate foam according to claim 7, characterized in that: The invention comprises the following raw materials in parts by weight: per 100 parts of acrylate monomer, 0.1-0.3 parts of initiator, 1-2 parts of crosslinking agent and 5-10 parts of antistatic heat expansion microspheres.
9. Use of the antistatic heat-expandable microspheres prepared by the method according to any one of claims 1 to 4 in polyacrylate foam.