A high-fluidity tea residue / polypropylene composite material and preparation method thereof
By using additives such as fluorine-containing flow modifiers and twin-screw extruder processing in tea residue/polypropylene composite materials, the problem of difficulty in balancing the mechanical properties and processing properties of tea plastic composite materials has been solved, and the melt index and melt index have been significantly improved. Processing fluidity, suitable for industrial production.
Patent Information
- Application Number
- CN202211686564.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-26
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2042-12-26
AI Technical Summary
When existing tea plastic composite materials improve the interface interaction between tea residue and polymer matrix, the processing viscosity of the composite material increases and the toughness decreases, making it difficult to balance the mechanical properties and processing performance.
Fluorine-containing flow modifiers, antioxidants, light stabilizers and antifungal agents are used to prepare high-flow tea residue/polypropylene composite materials through specific proportions and technological processes, and are processed using a twin-screw extruder to improve the composite Material melt index and processing flowability.
It is possible to significantly improve the melt index of composite materials while maintaining good mechanical strength and toughness, taking into account comprehensive performance and processing performance. It is suitable for industrial production and has economic and environmental benefits.
Smart Images

Figure CN116285407B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of composite materials, is a technical means for increasing the value of waste tea residues, and specifically relates to a high-fluidity tea residue / polypropylene composite material and a preparation method thereof. Background Art
[0002] In the process of annual tea making, deep processing of tea leaves (such as producing tea beverages, tea biscuits, etc.) and daily brewing of tea leaves by consumers, a large amount of tea residues (such as discarded tea dust, tea stems, tea byproducts, etc.) are produced, and its main components are cellulose and lignin, as well as a small amount of bioactive ingredients such as tea polyphenols, polysaccharides, and caffeine. At present, domestic tea residues produced in tea making, deep processing, and daily consumption processes are mostly discarded as waste, and only a small part is used as fuel and fertilizer. And the active substance content contained in the tea residues itself is low, resulting in high extraction cost, high difficulty, and low yield, and it is difficult to realize large-scale production. Therefore, how to fully develop and utilize the tea residues with a wide source, large output, and low cost is a key technology to further improve the income of tea farmers and tea companies, promote the benefits of the tea industry, and strengthen environmental protection construction.
[0003] Wood-plastic composites are a type of biomass composite material made by combining natural plant fibers with thermoplastic resins. They are stable, non-volatile, and recyclable, and are therefore considered green, healthy, and environmentally friendly composite materials. Research has found that the physical, chemical, and mechanical properties of tea dregs fibers can replace natural plant fibers such as wood powder, rice bran, and straw in wood-plastic composites. Tea-plastic composites prepared from tea dregs and thermoplastics are expected to achieve high-value utilization of tea dregs and become an important alternative in the wood-plastic composite industry (Journal of the Chinese Society of Agricultural Engineering, 2020, 36(18), 283-291).
[0004] Chinese Patent No. 201510971448.2 discloses a tea-plastic composite material and a preparation method thereof. The physical properties, mechanical properties and weather resistance of the invented tea-plastic composite material all meet or even exceed the index requirements in the national standard GB / T24508-2009 "Wood Plastic Flooring", and can meet market demand; Gong Xinhuai et al. (Plastic Industry, 2018, 46(3), 33-37) prepared tea residue / polypropylene composite materials using tea waste as raw materials, and explored the effects of different compatibilizers on the performance of the composite materials. Among them, maleic anhydride grafted polypropylene as a compatibilizer can effectively improve the interfacial compatibility between tea powder and polypropylene. When the mass fraction of tea powder reaches 50%, the tensile strength is increased by 17.6%. However, this interface modification method causes the melt index and impact strength of the composite material to decrease.
[0005] In summary, although the existing technology can prepare tea-plastic composite materials that meet market demand, traditional compatibilizers, while improving the interfacial interaction between tea residues and the polymer matrix, often lead to increased processing viscosity and decreased toughness of the composite materials, especially when the amount of tea residue added is high. The current tea-plastic composite materials still have the problem of difficulty in balancing good comprehensive performance and good processability. Summary of the invention
[0006] The present invention aims to solve one of the technical problems in the related art to at least a certain extent. To this end, the main purpose of the present invention is to provide a high-fluidity tea residue / polypropylene composite material, aiming to solve the problem that mechanical properties and processing properties cannot be taken into account in the prior art. The present invention also discloses a preparation method of the high-fluidity tea residue / polypropylene composite material.
[0007] The objective of the present invention is achieved through the following technical solutions:
[0008] In the first aspect, a high-fluidity tea residue / polypropylene composite material comprises, by mass percentage, 50% to 70% tea residue, 25% to 45% polypropylene, 1% to 3% fluorine-containing flow modifier, 1% to 2% antioxidant, 1% to 2% light stabilizer, and 0.5 to 1% mildewproofing agent.
[0009] Preferably, the particle size of the tea residue is 300-500 meshes.
[0010] Preferably, the fluorine-containing flow modifier is at least one of poly(hexafluorobutyl methacrylate-methyl methacrylate), poly(hexafluorobutyl methacrylate-styrene), and poly(hexafluorobutyl methacrylate-methyl methacrylate-styrene).
[0011] Furthermore, the fluorine-containing flow modifier is poly(hexafluorobutyl methacrylate-styrene).
[0012] Further, the poly(hexafluorobutyl methacrylate-styrene) is prepared by the following method:
[0013] In the reaction vessel, add the emulsifier solution, add equimolar amounts of the reaction monomers styrene and hexafluorobutyl methacrylate, raise the temperature to 75°C after pre-emulsification, stir at a rate of 250 rpm, add the initiator (NH 4 ) 2 S 2 O 8 ; After the addition, the emulsion was polymerized for 4 hours and cooled to room temperature; the emulsion was heated to 70°C and Al 2 (SO 4 ) 3The solution was demulsified; the mixed emulsion was separated into layers, filtered, washed, and dried in a vacuum oven at 50° C. for 24 hours to obtain a white powder, namely poly(hexafluorobutyl methacrylate-styrene).
[0014] Preferably, the antioxidant is at least one of antioxidant 1010, antioxidant 1076, antioxidant 264, antioxidant BHT, and antioxidant TNP.
[0015] Preferably, the light stabilizer is at least one of light stabilizer AM-101, light stabilizer GW-540, light stabilizer 944, light stabilizer 744, ultraviolet absorber UV-326, and ultraviolet absorber UV-531.
[0016] Preferably, the mildew preventer is at least one of LF-053, wood plastic mildew preventer JL-1069, and wood plastic mildew preventer Irgaguard F3000.
[0017] In a second aspect, a method for preparing the aforementioned high-fluidity tea residue / polypropylene composite material comprises the following steps:
[0018] 1) Pretreatment of tea residues: crushing and sieving the fully dried tea residues using a crusher;
[0019] 2) Mixing: according to the formula requirements, tea residues, polypropylene, fluorinated flow modifier, antioxidant, light stabilizer and mildew inhibitor are put into a mixer and mixed evenly to obtain a mixture;
[0020] 3) Extrusion granulation: the mixed material obtained in step 2) is added into a twin-screw extruder to extrude into strips and cut into pellets, and then dried to obtain a high-fluidity tea residue / polypropylene composite material.
[0021] Furthermore, the temperature of the twin-screw extruder in step (3) is: 160-170°C in zone 1, 170-190°C in zone 2, 180-200°C in zone 3, 180-200°C in zone 4, 180-200°C in zone 5, 170-190°C in zone 6, the main engine speed is 150-250r / min, and the feed speed is 8-15r / min.
[0022] Compared with the prior art, the present invention has at least the following advantages:
[0023] 1) The high-fluidity tea residue / polypropylene composite material provided by the present invention adopts the selective interface distribution property of the fluorine-containing flow modifier with low surface energy, so that a specific proportion of the tea residue / polypropylene composite material is distributed at the interface between the tea residue and the polypropylene during the melt extrusion process, which not only plays a role in dispersing the tea residue, but also effectively reduces the friction resistance between the tea residues, thereby improving the processing flowability of the composite material; combined with other technical features in the composite material, the melt index of the tea residue / polypropylene composite material is improved by more than 3 times while maintaining good mechanical strength and toughness, taking into account the good comprehensive performance and processability of the tea residue / polypropylene composite material, conforming to the sustainable development policy, and having obvious economic and environmental benefits.
[0024] 2) The preparation method of the high-fluidity tea residue / polypropylene composite material provided by the present invention has simple process, strong plantability and is suitable for industrial production. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] In order to more clearly illustrate the specific embodiments of the present invention, the drawings required for use in the specific embodiments or the description of the prior art will be briefly introduced below.
[0026] Figure 1 is the nuclear magnetic resonance spectrum of the fluorinated flow modifier-poly(hexafluorobutyl methacrylate-styrene) in the present invention; DETAILED DESCRIPTION
[0027] The present invention will be further described in detail below in conjunction with the accompanying drawings and embodiments. The following embodiments are only illustrative and not restrictive, and the protection scope of the present invention cannot be limited thereto.
[0028] When a certain amount, concentration or other value or parameter is expressed in the form of a range, a preferred range, or a preferred upper and lower numerical limit, it should be understood that it is equivalent to specifically revealing any range by combining any pair of upper range limits or preferred numerical values with any lower range limit or preferred numerical value, regardless of whether the range is specifically disclosed. Unless otherwise indicated, the numerical range values listed herein include the endpoints of the range, and all integers and fractions within the range.
[0029] Unless otherwise indicated, all percentages, parts, ratios, etc. herein are by weight.
[0030] The materials, methods, and examples herein are illustrative and are not to be construed as limiting unless specifically stated.
[0031] Unless otherwise specified, the professional and scientific terms used herein have the same meanings as those familiar to those skilled in the art. In addition, any method or material similar or equivalent to the described content can also be applied to the present invention. The experimental methods without specifying specific conditions in the examples are usually carried out under conventional conditions or under conditions recommended by the manufacturer.
[0032] In the following embodiments:
[0033] The tea residues used are the discarded tea dust and tea stems in the production process of Chaozhou Phoenix Dancong tea;
[0034] The fluorinated flow modifier in the present application is at least one of poly(hexafluorobutyl methacrylate-methyl methacrylate), poly(hexafluorobutyl methacrylate-styrene), and poly(hexafluorobutyl methacrylate-methyl methacrylate-styrene). The present application takes the fluorinated flow modifier of poly(hexafluorobutyl methacrylate-styrene) as an example to illustrate its synthesis method: in a four-necked bottle equipped with a stirrer, a condenser, and a constant pressure dropping funnel, add 80 mL of emulsifier solution (a deionized water solution of sodium dodecyl sulfate and octylphenol polyoxyethylene ether in a mass ratio of 1:1, and the mass concentration of the emulsifier solution is 0.5%), add 6.2 g of styrene and 15 g of hexafluorobutyl methacrylate, stir at room temperature for 30 minutes for pre-emulsification, and the stirring rate is 400 rpm, and then heat to 75°C in an oil bath pot, stir at a rate of 250 rpm, and add 10 mL of initiator solution (initiator (NH 4 ) 2 S 2 O 8 The mass concentration is 1%), and the emulsion polymerization reaction is carried out for 4 hours after dropwise addition, and then cooled to room temperature; the above emulsion is added to a three-necked flask, and the temperature is raised to 70°C. At a stirring rate of 150rpm, 200mLAl is added through a constant pressure dropping funnel. 2 (SO 4 ) 3 The solution (the mass concentration of the solution is 5%) is subjected to demulsification treatment; the mixed emulsion is separated into layers, the filtrate is filtered to remove the filtrate, the filter residue is collected, the filter residue is washed with excess deionized water, and dried in a vacuum oven at 50° C. for 24 hours to obtain a white powder.
[0035] The white powder obtained was treated with 1 HNMR characterization results are as follows Figure 1 As shown in the figure, the chemical shift peaks in the NMR spectrum correspond well to the hydrogen atoms in the molecular structure. The chemical shift at 2.5 ppm is the characteristic peak of deuterated DMSO solvent. 3 ) corresponds to a chemical shift of 0.86 ppm, and the methylene (-CH 2-) corresponds to the chemical shifts of 1.67 ppm and 1.92 ppm, while -O-CH 2 -Hydrogen atoms on the benzene ring of polystyrene correspond to chemical shifts of 4.65-4.72 ppm, and hydrogen atoms on the benzene ring of polystyrene correspond to chemical shifts of 6.5-7.5 ppm. Combined with the fact that the monomers used in this example are all liquid, the final product is a white solid powder, indicating the successful synthesis of poly(hexafluorobutyl methacrylate-styrene).
[0036] Example 1
[0037] The high-fluidity tea residue / polypropylene composite material provided by the present invention is prepared by the following method:
[0038] (1) Pretreatment of tea residue: Use a small pulverizer to pulverize the waste tea residue and tea stems with a moisture content of less than 5%, and then process them through a 300-mesh screen and dry them for later use;
[0039] (2) Mixing: 50% of pretreated tea residue, 45% of polypropylene pellets (PP), 1% of fluorinated flow modifier, 1.5% of antioxidant, 2% of light stabilizer, and 0.5% of mildew inhibitor were added into a mixer according to the mass percentage, with a rotation speed of 100 r / min and a mixing time of 20 min;
[0040] (3) Extrusion granulation: The mixed material obtained in step (2) is added into a twin-screw extruder, and extruded into strips according to the set temperatures: zone 1 160°C, zone 2 170°C, zone 3 180°C, zone 4 180°C, zone 5 180°C, zone 6 170°C, main engine speed 150 r / min, feed speed 8 r / min, and then water-cooled, blow-dried, pelletized and dried to obtain a high-flow tea residue / polypropylene composite material.
[0041] The antioxidant in the present application is antioxidant 1010; the light stabilizer is light stabilizer AM-101; and the mildew preventer is wood plastic mildew preventer LF-053.
[0042] Example 2
[0043] The high-fluidity tea residue / polypropylene composite material provided by the present invention is prepared by the following method:
[0044] (1) Pretreatment of tea residue: Use a small pulverizer to pulverize the fully dried waste tea residue and tea stems, and then process them through a 400-mesh screen and dry them for later use;
[0045] (2) Mixing: 70% of pretreated tea residue, 25% of polypropylene pellets (PP), 2% of fluorinated flow modifier, 1% of antioxidant, 1% of light stabilizer, and 1% of mildew inhibitor were added into a mixer according to the mass percentage, with a rotation speed of 100 r / min and a mixing time of 20 min;
[0046] (3) Extrusion granulation: The mixed material obtained in step (2) is added into a twin-screw extruder, and extruded into strips according to the set temperatures: zone 1 170°C, zone 2 190°C, zone 3 200°C, zone 4 200°C, zone 5 200°C, zone 6 190°C, main engine speed 250 r / min, feed speed 15 r / min, and then water-cooled, blow-dried, pelletized and dried to obtain a high-flow tea residue / polypropylene composite material.
[0047] The antioxidant in the present application is a mixture of antioxidant 1010 and antioxidant 264 in a mass ratio of 1:1; the light stabilizer is light stabilizer 944; and the mildew inhibitor is wood plastic mildew inhibitor JL-1069.
[0048] Example 3
[0049] The high-fluidity tea residue / polypropylene composite material provided by the present invention is prepared by the following method:
[0050] (1) Pretreatment of tea residue: Use a small pulverizer to pulverize the fully dried waste tea residue and tea stems, and then process them through a 500-mesh screen and dry them for later use;
[0051] (2) Mixing: 60% of pretreated tea residue, 35% of polypropylene pellets (PP), 3% of fluorinated flow modifier, 1% of antioxidant, 0.5% of light stabilizer, and 0.5% of mildew inhibitor were added into a mixer according to the mass percentage, with a rotation speed of 100 r / min and a mixing time of 20 min;
[0052] (3) Extrusion granulation: The mixed material obtained in step (2) is added into a twin-screw extruder, and extruded into strips according to the set temperatures: zone 1 170°C, zone 2 190°C, zone 3 200°C, zone 4 200°C, zone 5 200°C, zone 6 190°C, main engine speed 250 r / min, feed speed 15 r / min, and then water-cooled, blow-dried, pelletized and dried to obtain a high-flow tea residue / polypropylene composite material.
[0053] The antioxidant in the present application is antioxidant BHT; the light stabilizer is ultraviolet absorber UV-326; and the mildew preventer is wood plastic mildew preventer Irgaguard F3000.
[0054] Comparative Example 1
[0055] The tea residue / polypropylene composite material provided in this comparative example is different from that in Example 3 only in that maleic anhydride grafted polypropylene (MAPP) is used to replace the fluorinated flow modifier.
[0056] Comparative Example 2
[0057] The tea residue / polypropylene composite material provided in this comparative example is different from that in Example 3 only in that no fluorinated flow modifier is added.
[0058] Comparative Example 3
[0059] The tea residue / polypropylene composite material provided in this comparative example is different from that in Example 3 only in that a fluorine-containing flow modifier is used, which is poly(hexafluorobutyl methacrylate).
[0060] Performance Testing:
[0061] The present application performs performance tests on the tea residue / polypropylene composite materials provided in Examples 1-3 and Comparative Examples 1-3, wherein: in order to test the mechanical properties of the composite materials, standard test specimens are injection molded by an injection molding machine, the injection molding temperature is 170-190°C, and the injection molding pressure is 45-65MPa; the preparation conditions of the test specimens in each embodiment and comparative example are the same.
[0062] The tensile properties of the composite materials were tested according to GB / T1040-1992, the impact strength of the composite materials was tested according to GB / T1843-2008, and the melt index of the composite materials was tested according to GB / T3682-2000. The specific test results are shown in Table 1:
[0063] Table 1. Performance test results of tea residue / PP composite materials prepared in Examples 1-3 and Comparative Examples 1-3
[0064] Example 1 Example 2 Example 3 Comparative Example 1 Comparative Example 2 Comparative Example 3 Tensile strength(MPa) 16.15 15.52 15.24 20.99 13.21 14.59 <![CDATA[Impact strength KJ / m 2 > 1.41 1.36 1.43 0.92 1.12 1.23 Melt index g / 10min 6.99 7.37 8.24 2.61 2.04 3.26
[0065] As can be seen from Table 1, by comparing Example 3 with Comparative Example 1, after the introduction of MAPP compatibilizer in the tea residue / polypropylene composite material, the tensile strength is improved while the impact strength is reduced, that is, MAPP can improve the interfacial interaction between tea residue and PP, and the strength is improved while the toughness is deteriorated. By comparing Example 3 with Comparative Example 3, it can be seen that by introducing a common fluorinated flow agent (hexafluorobutyl polymethacrylate) into the tea residue / polypropylene composite material, the tensile strength and impact strength are improved, but the melt index is improved to a limited extent; and after the introduction of the fluorinated flow modifier, the tensile strength of the tea residue / polypropylene composite material of the present application is improved, and the impact strength is also increased and the toughness is improved; at the same time, after the introduction of the fluorinated flow modifier, the melt index of the composite material is increased by more than 3 times, indicating that its processing fluidity has been significantly improved, effectively solving the problem that the tea-plastic composite material is difficult to take into account both good comprehensive performance and good processability.
[0066] Example 4
[0067] The preparation method of the high-flow tea residue / polypropylene composite material provided in this embodiment is different from that in Example 3 in that the fluorinated flow modifier used is poly(hexafluorobutyl methacrylate-methyl methacrylate) or poly(hexafluorobutyl methacrylate-methyl methacrylate-styrene). Performance tests were conducted on the composite material, and the results showed that the tensile strength, impact strength and melt index were comparable to those in Example 3.
[0068] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein by equivalents. These modifications or replacements do not make the essence of the corresponding technical solutions deviate from the scope of the technical solutions of the embodiments of the present invention, and they should all be included in the scope of the claims and specification of the present invention.
Claims
1. A high-fluidity tea residue / polypropylene composite material, characterized in that: The invention comprises, by mass percentage, 50% to 70% of tea residues, 25% to 45% of polypropylene, 1% to 3% of a fluorine-containing flow modifier, 1% to 2% of an antioxidant, 1% to 2% of a light stabilizer, and 0.5% to 1% of a mildewproofing agent; wherein the fluorine-containing flow modifier is poly(hexafluorobutyl methacrylate-styrene).
2. The high-fluidity tea residue / polypropylene composite material according to claim 1, characterized in that: The particle size of the tea residue is 300-500 meshes.
3. The high-fluidity tea residue / polypropylene composite material according to claim 1 or 2, characterized in that: The poly(hexafluorobutyl methacrylate-styrene) is prepared by the following method: In a reaction vessel, add an emulsifier solution, add equimolar amounts of reactive monomers styrene and hexafluorobutyl methacrylate, heat to 75°C after pre-emulsification, stir at a rate of 250rpm, add initiator (NH4)2S2O8; after dropwise addition, emulsion polymerization is carried out for 4 hours, and then cooled to room temperature; the emulsion is heated to 70°C and demulsified by adding Al2(SO4)3 solution; the mixed emulsion is separated into layers, filtered, washed, and dried in a vacuum oven at 50°C for 24 hours to obtain a white powder, namely poly(hexafluorobutyl methacrylate-styrene).
4. The high-fluidity tea residue / polypropylene composite material according to claim 1, characterized in that: The antioxidant is at least one of antioxidant 1010, antioxidant 1076, antioxidant 264, antioxidant BHT, and antioxidant TNP.
5. The high-fluidity tea residue / polypropylene composite material according to claim 1, characterized in that: The light stabilizer is at least one of light stabilizer AM-101, light stabilizer GW-540, light stabilizer 944, light stabilizer 744, ultraviolet absorber UV-326, and ultraviolet absorber UV-531.
6. The high-fluidity tea residue / polypropylene composite material according to claim 1, characterized in that: The mildew preventer is at least one of wood plastic mildew preventer LF-053, wood plastic mildew preventer JL-1069, and wood plastic mildew preventer Irgaguard F3000.
7. A method for preparing the high-fluidity tea residue / polypropylene composite material according to any one of claims 1 to 6, characterized in that: The steps include: 1) Pretreatment of tea residues: crushing and sieving the fully dried tea residues using a crusher; 2) Mixing: according to the formula requirements, tea residue, polypropylene, fluorine-containing flow modifier, antioxidant, light stabilizer and mildew inhibitor are put into a mixer and mixed evenly to obtain a mixture; 3) Extrusion granulation: the mixed material obtained in step 2) is added into a twin-screw extruder to extrude into strips and cut into pellets, and then dried to obtain a high-fluidity tea residue / polypropylene composite material.
8. The method for preparing the high-fluidity tea residue / polypropylene composite material according to claim 7, characterized in that: The temperature of the twin-screw extruder in step (3) is: 160-170°C in zone 1, 170-190°C in zone 2, 180-200°C in zone 3, 180-200°C in zone 4, 180-200°C in zone 5, 170-190°C in zone 6, the main engine speed is 150-250r / min, and the feed speed is 8-15r / min.