A water-based polymer coating for wiper blades and its use method and application

The water-based polymer coating composed of modified water-based polyurethane dispersion and solid lubricant solves the problem of high friction resistance of the wiper blade in the wet state and dry-to-wet transition state, achieving low friction and high water resistance, reducing It reduces noise and vibration and avoids contamination by organic solvents. It is suitable for wiper blades made of neoprene rubber.

CN116285635BActive Publication Date: 2024-10-18SHANGHAI LANOU CHEM IND TECH
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202310305316.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-03-27
Publication Date
2024-10-18
Estimated Expiration
2043-03-27

AI Technical Summary

Technical Problem

Existing wiper blade coatings have greater frictional resistance in the wet state and the wet-dry transition state, resulting in increased wiper noise and vibration, and contain organic solvents, which poses pollution problems.

Method used

A water-based polymer coating composed of modified water-based polyurethane dispersion, solid lubricant and deionized water is used to prepare a network-shaped cross-linked polyurethane polymer through cross-linking modification technology to form a low friction coefficient coating. Suitable for wiper blades to reduce friction between the strip and the glass.

Benefits of technology

The surface friction coefficient is lower than 0.2 in dry, wet and semi-wet states, which significantly reduces the friction between the wiper blade and the glass, improves the bonding strength and water resistance, reduces noise and shaking, and at the same time It avoids the pollution of organic solvents and is suitable for industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004146543260000041
    Figure BDA0004146543260000041
  • Figure BDA0004146543260000042
    Figure BDA0004146543260000042
  • Figure BDA0004146543260000051
    Figure BDA0004146543260000051
Patent Text Reader

Abstract

The present application relates to the technical field of wipers, and in particular to a water-based polymer coating for wiper blades, and its use method and application. The coating is composed of the following components in parts by weight: 40-60 parts of modified aqueous polyurethane dispersion, 3-5 parts of dispersant, 8-12 parts of solid lubricant, 8-10 parts of polydimethylsiloxane, 0.9-1.8 parts of functional additives, and 18-22 parts of deionized water; the modified aqueous polyurethane dispersion is synthesized from polycarbonate diol, isophorone diisocyanate and polysiloxane; wherein the polysiloxane is selected from one or more of terminal hydroxyl polydimethylsiloxane, carbon hydroxyl-terminated polydimethylsiloxane and N-(β-aminoethyl)-γ-aminopropyltrimethoxysilane. The coating prepared by the above components in the present application has good lubricity and wear resistance, and can effectively reduce the friction between the rubber strip and the windshield after being applied to the wiper blade.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of windshield wipers, and more specifically, to a water-based polymer coating for a windshield wiper blade and a use method and application thereof. Background Art

[0002] Wipers are important components used to remove water stains on the windshield surface to ensure driving vision. Their quality is of great significance to driving safety. However, in daily use, the friction of wiper blades will gradually increase with the frequency of use. In severe cases, the wiper blades and / or the wiper system may be damaged.

[0003] Therefore, a special coating applied to the contact part between the wiper blade and the glass to reduce the friction between the two has come into being. In the relevant technology, the special coating for wiper blades mainly adopts the following schemes:

[0004] The invention is made of graphite and dimethyl silicone oil as main components, and is mixed with one or more of polyol resin, urethane resin, hydroxyl-containing fluororesin, epoxy resin and silicone resin in the presence of an organic solvent. When used, it can effectively reduce the noise and shaking of wipers.

[0005] However, the above-mentioned coating will produce greater friction resistance in wet state and dry-wet conversion state, which significantly aggravates the noise and shaking of the wiper. In addition, the organic solvent is selected from butanone, xylene and butyl acetate, which has certain pollution. Therefore, a water-based polymer material synthetic coating material for automobile windshield CR wiper blade and its use method and application are specially provided. Summary of the invention

[0006] In order to reduce the friction coefficient between the wiper blade and the glass under different wiping frequencies such as dry state, wet state and dry-wet transition state, thereby reducing the problem of large scraping resistance under different scraping states, the present application specially provides a water-based polymer synthetic coating material for automobile windshield CR wiper blades.

[0007] In a first aspect, the present application provides a water-based polymer coating for a wiper blade, which adopts the following technical solution:

[0008] A water-based polymer coating for a wiper blade, comprising the following components in parts by weight:

[0009] 40-60 parts of modified waterborne polyurethane dispersion, 3-5 parts of dispersant, 8-12 parts of solid lubricant, 8-10 parts of polydimethylsiloxane, 0.9-1.8 parts of functional additives, and 18-22 parts of deionized water;

[0010] The modified aqueous polyurethane dispersion is synthesized from polycarbonate diol, isophorone diisocyanate and polysiloxane; wherein the polysiloxane is selected from one or more of terminal hydroxyl polydimethylsiloxane, carbon hydroxyl-terminated polydimethylsiloxane and N-(β-aminoethyl)-γ-aminopropyltrimethoxysilane.

[0011] By adopting the above technical solution, the water-based polymer coating obtained has a water absorption rate of ≤1.5% / 72h after film formation, and the surface friction coefficients of dry, wet and semi-wet states are all ≤0.2, so after being applied to wiper blades, the friction between the rubber strip and the windshield can be effectively reduced;

[0012] The possible reason is that the modified waterborne polyurethane dispersion used uses polycarbonate diol as the soft segment, isophorone diisocyanate (IPDI) as the hard segment, and polysiloxane as the cross-linked modified segment to synthesize a network cross-linked polyurethane polymer. Thanks to the large number of active groups contained in it, it has excellent bonding strength and water resistance after curing, and can thus meet various application requirements of wiper blades.

[0013] Preferably, the synthesis method of the modified waterborne polyurethane resin is as follows:

[0014] S1. Prepolymer synthesis: polycarbonate diol, excess isophorone diisocyanate and catalyst DBTDL are prepolymerized in DMF solution at 50-60° C. for 10-15 h in a nitrogen atmosphere, and dried to obtain a prepolymer;

[0015] S2. Cross-linking modification: Add cross-linking agent TMP and polysiloxane to the prepolymer, and react at 70-80° C. for 40-56 hours in a nitrogen atmosphere to obtain a modified waterborne polyurethane resin dispersion.

[0016] Preferably, the usage ratio of polycarbonate diol, isophorone diisocyanate and catalyst in S1 is 1:(2.4-3.6):(0.005-0.008).

[0017] Preferably, the usage ratio of the prepolymer, the crosslinking agent TMP and the polysiloxane in S2 is 1:(0.2-0.3):(0.3-0.5).

[0018] Preferably, the polysiloxane is composed of hydroxyl-terminated polydimethylsiloxane, carbon hydroxyl-terminated polydimethylsiloxane and N-(β-aminoethyl)-γ-aminopropyltrimethoxysilane.

[0019] Preferably, the polysiloxane is composed of hydroxyl-terminated polydimethylsiloxane, carbon hydroxyl-terminated polydimethylsiloxane and N-(β-aminoethyl)-γ-aminopropyltrimethoxysilane in a weight ratio of 1:(1-2):(0.5-0.8).

[0020] By adopting the above technical solution, the prepared modified waterborne polyurethane dispersion has more complete cross-linking modification effect of each component, has extremely excellent adhesion effect and water resistance, and still has low scratch resistance in wet and semi-wet states, which can effectively meet the performance requirements of wiper blade coatings;

[0021] The possible reason is that the carbon hydroxyl-modified polydimethylsiloxane, N-(β-aminoethyl)-γ-aminopropyltrimethoxysilane and terminal hydroxyl polydimethylsiloxane undergo more complete multiple cross-linking reactions with the polyurethane components, and the hydrophobicity, scratch resistance and adhesion of the copolymer can be significantly improved through further reaction of the active carbon hydroxyl groups in the copolymer with the active groups in the polyurethane.

[0022] Preferably, the solid lubricant is selected from one or more of molybdenum disulfide, graphite and boron nitride.

[0023] Preferably, the functional additive consists of a wetting agent, a leveling agent and a defoaming agent.

[0024] In a second aspect, the present application provides a method for using a water-based polymer coating for a wiper blade, which adopts the following technical solution:

[0025] A method for using a water-based polymer coating for a wiper blade, the specific steps are as follows:

[0026] Weigh the above raw materials in proportion, mix and stir until fully uniform, spray them on both sides of the wiper blade edge, and then cure them at 100-120°C for 5-15 minutes and then cool them.

[0027] On the third aspect, the present application provides an application of a water-based polymer coating for wiper blades, which is particularly suitable for wiper blades and materials made of chloroprene rubber.

[0028] In summary, this application has the following beneficial effects:

[0029] 1. The water-based polymer coating prepared from the above components in this application has a water absorption rate of ≤1.5% / 72h after film formation, and the surface friction coefficients of dry, wet and semi-wet states are all ≤0.2, so it can effectively reduce the friction between the wiper blade and the windshield after being applied to the wiper blade;

[0030] 2. The aqueous polyurethane dispersion used in the present application has excellent adhesion and water resistance after being modified by increasing molecular weight, hydrophobicity and multiple cross-linking, and thus still has low scratch resistance in wet and semi-wet states;

[0031] 3. The water-based polymer coating developed in this application is particularly suitable for wiper blades and materials made of chloroprene rubber. After curing, it can form a lubricating coating with excellent bonding strength and excellent wear resistance, which can reduce friction during operation without generating noise. The preparation method and usage method are simple and clear, and the raw materials are green and pollution-free, which is suitable for industrial production. DETAILED DESCRIPTION

[0032] The present application is further described in detail below in conjunction with the examples. Except for the following special instructions, the raw materials used are all common commercially available materials:

[0033] Product Name Brand / Specification Supramolecular dispersants American Gas Molybdenum disulfide powder 2500 mesh graphite 5000 mesh High molecular weight polydimethylsiloxane Dow Corning Wetting Agents Dow Corning DC51 Leveling agent Digo Defoaming agent DC65

[0034] Preparation Example

[0035] Preparation Example 1

[0036] A waterborne polyurethane dispersion, the synthesis method of which is as follows:

[0037] S1. Prepolymer synthesis: polycarbonate diol, isophorone diisocyanate and catalyst DBTDL were prepolymerized in a 30% DMF solution at 50° C. for 15 h in a nitrogen atmosphere and dried for 1 h to obtain a prepolymer;

[0038] The dosage ratio of polycarbonate diol, isophorone diisocyanate and catalyst is 1:2:0.005.

[0039] S2, cross-linking modification: adding a cross-linking agent TMP and polysiloxane to the prepolymer, reacting at 70° C. for 56 hours in a nitrogen atmosphere to obtain a modified waterborne polyurethane resin dispersion;

[0040] The usage ratio of prepolymer, crosslinking agent TMP and polysiloxane is 1:0.1:0.2; the polysiloxane is terminal hydroxyl polydimethylsiloxane.

[0041] Preparation Example 2

[0042] An aqueous polyurethane dispersion, which differs from Preparation Example 1 in that the synthesis method is as follows:

[0043] S1. Prepolymer synthesis: polycarbonate diol, isophorone diisocyanate and catalyst DBTDL were prepolymerized in a 30% DMF solution at 58° C. for 12 h in a nitrogen atmosphere and dried for 1 h to obtain a prepolymer.

[0044] S2. Cross-linking modification: Add a cross-linking agent TMP and polysiloxane to the prepolymer, and react at 75° C. for 48 hours in a nitrogen atmosphere to obtain a modified waterborne polyurethane resin dispersion.

[0045] Preparation Example 3

[0046] An aqueous polyurethane dispersion, which differs from Preparation Example 1 in that the synthesis method is as follows:

[0047] S1. Prepolymer synthesis: polycarbonate diol, isophorone diisocyanate and catalyst DBTDL were prepolymerized in a 30% DMF solution at 60° C. for 10 h in a nitrogen atmosphere and dried for 1 h to obtain a prepolymer.

[0048] S2. Cross-linking modification: Add a cross-linking agent TMP and polysiloxane to the prepolymer, and react at 80° C. for 40 hours in a nitrogen atmosphere to obtain a modified waterborne polyurethane resin dispersion.

[0049] Preparation Example 4-7

[0050] An aqueous polyurethane dispersion, which differs from Preparation Example 1 in that the proportions of raw materials used for the prepolymer in S1 are different, as shown in the following table:

[0051]

[0052] Preparation Example 8-11

[0053] An aqueous polyurethane dispersion, which differs from Preparation Example 5 in that the proportions of the raw materials used in S2 are different, as shown in the following table:

[0054]

[0055]

[0056] Preparation Examples 12-16

[0057] An aqueous polyurethane dispersion, which differs from Preparation Example 9 in that the use of polysiloxane in S2 is different, as shown in the following table:

[0058]

[0059] The performance test selected the wiper blade coatings prepared in the following embodiments and / or comparative examples as test objects, and tested the water absorption rate, friction coefficient and bench scraping times after film formation respectively. The sample conditions are as follows:

[0060] Sample conditions to be tested: Spray the tested coating on both sides of the blade of the wiper (chloroprene rubber material) (coating thickness 15±1um), then cure at 120℃ for 10 minutes and cool down;

[0061] The reference testing standards are as follows:

[0062] 1) Water absorption after film formation (% / 72h) refers to HG / T 3344-1985 "Determination of water absorption of paint film";

[0063] 2) Friction coefficient (dry, wet, dry and wet) refer to GB / T 10006-1988 "Determination of friction coefficient of plastic films and sheets";

[0064] 3) The number of times the bench is scraped shall refer to QC / T 44-2009 "Electric Wiper for Automobile Windshield". It is considered qualified if it can be wiped more than 500,000 times without defects such as falling off, shaking, water lines, abnormal noise, etc.

[0065] Example

[0066] Examples 1-5

[0067] A water-based polymer coating for a wiper blade, the raw material components and dosage thereof are shown in the following table (kg):

[0068] Table: Raw material components and their weights in Examples 1-5 (kg)

[0069]

[0070] The modified aqueous polyurethane dispersion is prepared by Preparation Example 1;

[0071] The dispersant is a supramolecular dispersant purchased from American Gas;

[0072] The solid lubricant is composed of molybdenum disulfide powder and graphite in a weight ratio of 1.5:1;

[0073] Dimethicone is a high molecular weight polydimethylsiloxane (Dow Corning);

[0074] The functional additives are composed of a wetting agent (Dow Corning DC51), a leveling agent (Digo) and a defoaming agent (DC65) in a weight ratio of 1:1:1.

[0075] Comparative Example 1

[0076] A coating for wiper blades, which is different from Example 1 in that the modified aqueous polyurethane dispersion in the preparation raw material is replaced by an equal amount of aqueous polyurethane dispersion (solid content 51%, anionic, viscosity 25°C 2600 cPs).

[0077] Comparative Example 2

[0078] A coating for wiper blades, which is different from Example 1 in that the modified aqueous polyurethane dispersion in the preparation raw material is replaced by an equal amount of aqueous acrylic resin dispersion (solid content 45%, hydroxyl content 3.5% based on solids).

[0079] Comparative Example 3

[0080] A coating for wiper blades, which is different from Example 1 in that the modified aqueous polyurethane dispersion in the preparation raw material is replaced by an equal amount of aqueous epoxy resin dispersion (solid content 53%, epoxy equivalent 450-550 g / mol).

[0081] The coatings prepared in the above Examples 1-5 and Comparative Examples 1-3 were selected as test objects, and then their water absorption rate, friction coefficient and number of bench scratches after film formation were tested according to the above test standards. The specific test results were averaged and recorded in the following table.

[0082] Table: Performance test results of Examples 1-5 and Comparative Examples 1-3

[0083]

[0084] As can be seen from the above table, the water-based polymer coatings for wiper blades obtained in Examples 1-5 all have excellent water resistance and scratch resistance after curing, and the water absorption rate after film formation is ≤1.5% / 72h, the surface friction coefficient (dry state, wet state and semi-wet state) is ≤0.15, and the number of bench scratches is all qualified;

[0085] It can be seen that the above-mentioned water-based polymer coating can effectively reduce the friction between the wiper blade and the windshield after being applied to the wiper blade. Compared with comparative examples 1-3 (conventional groups on the market), its application value and test performance are significantly improved. The reasons may be analyzed as follows: the modified water-based polyurethane dispersion used uses polycarbonate diol as the soft segment, isophorone diisocyanate as the hard segment, and polysiloxane as the cross-linking modified segment to synthesize a network cross-linked polyurethane polymer. Benefiting from the large number of active groups contained therein, it has excellent bonding strength and water resistance after curing.

[0086] It can also be seen from the data of Examples 1-5 that the preferred components and amounts are as shown in the table above, and any adjustment within the above range is not likely to interfere with the performance of the actual product, which is conducive to ensuring the stability of the quality of the finished product and is more suitable for industrial processing and production.

[0087] In addition, it can be seen from Comparative Examples 1-3 that the above-mentioned coating will produce greater friction resistance in the wet state and the dry-wet conversion state due to the swelling of the coating (resin component) due to water absorption, which significantly aggravates the noise and shaking of the wiper, which is not conducive to the operation of the wiper and the control of the drive system.

[0088] Embodiment 6-7

[0089] A water-based polymer coating for a wiper blade is different from Example 1 in that the modified waterborne polyurethane dispersion used is used differently, and the specific corresponding relationship is shown in the following table.

[0090] Table: Comparison table of usage of modified waterborne polyurethane dispersion in Examples 6-7

[0091] Group Modified waterborne polyurethane dispersion Example 6 Prepared from Preparation Example 2 Example 7 Prepared from Preparation Example 3

[0092] Embodiment 8-11

[0093] A water-based polymer coating for a wiper blade is different from Example 1 in that the modified waterborne polyurethane dispersion used is used differently, and the specific corresponding relationship is shown in the following table.

[0094] Table: Comparison table of usage of modified waterborne polyurethane dispersion in Examples 8-11

[0095] Group Modified waterborne polyurethane dispersion Example 8 Prepared by Preparation Example 4 Example 9 Prepared from Preparation Example 5 Example 10 Prepared from Preparation Example 6 Embodiment 11 Prepared from Preparation Example 7

[0096] Examples 12-15

[0097] A water-based polymer coating for a wiper blade is different from Example 9 in that the usage of the modified waterborne polyurethane dispersion is different. The specific corresponding relationship is shown in the following table.

[0098] Table: Comparison table of usage of modified waterborne polyurethane dispersion in Examples 12-15

[0099] Group Modified waterborne polyurethane dispersion Example 12 Prepared from Preparation Example 8 Embodiment 13 Prepared from Preparation Example 9 Embodiment 14 Prepared from Preparation Example 10 Embodiment 15 Prepared from Preparation Example 11

[0100] Examples 16-20

[0101] A water-based polymer coating for a wiper blade, which is different from Example 13 in that the modified aqueous polyurethane dispersion used is used differently, and the specific corresponding relationship is shown in the following table.

[0102] Table: Comparison table of usage of modified waterborne polyurethane dispersion in Examples 16-20

[0103] Group Modified waterborne polyurethane dispersion Example 16 Prepared from Preparation Example 12 Embodiment 17 Prepared from Preparation Example 13 Embodiment 18 Prepared from Preparation Example 14 Embodiment 19 Prepared from Preparation Example 15 Embodiment 20 Prepared from Preparation Example 16

[0104] The coatings prepared in Examples 6-20 were selected as test objects, and then their water absorption, friction coefficient and number of bench scratches after film formation were tested according to the above test standards. The specific test results were averaged and recorded in the following table.

[0105] Table: Performance test results of Examples 1, 6-20

[0106]

[0107]

[0108] As can be seen from the above table, the water-based polymer coatings for the wiper blades obtained in Examples 1, 6-20 all have excellent water resistance and scratch resistance after curing, and the water absorption rate after film formation is ≤1.5% / 72h, the surface friction coefficient (dry state, wet state and semi-wet state) is ≤0.15, and the number of bench scratches is all qualified;

[0109] It can be seen that the modified waterborne polyurethane dispersion prepared under the above conditions has a more complete cross-linking modification effect of each component, has extremely excellent adhesion and water resistance, and still has low scratch resistance in wet and semi-wet states, which can effectively meet the performance requirements of wiper blade coatings;

[0110] It can be seen from Examples 1, 6-7 that the preferred synthesis process of the modified waterborne polyurethane resin is as follows:

[0111] S1. Prepolymer synthesis: polycarbonate diol, excess isophorone diisocyanate and catalyst DBTDL are prepolymerized in DMF solution at 50-60° C. for 10-15 h in a nitrogen atmosphere, and dried to obtain a prepolymer;

[0112] S2. Cross-linking modification: Add cross-linking agent TMP and polysiloxane to the prepolymer, and react at 70-80° C. for 40-56 hours in a nitrogen atmosphere to obtain a modified waterborne polyurethane resin dispersion.

[0113] Any adjustment of the parameter conditions within the above range will not cause fluctuations in the performance of the actual product. The operation is convenient and easy to control the stability of the conditions and the quality of the finished product, and the industrialization value is extremely high.

[0114] It can also be seen from Examples 1 and 8-11 that the preferred dosage ratio of polycarbonate diol, isophorone diisocyanate and catalyst is 1:(2.4-3.6):(0.005-0.008). Within this range, the compounding effect of each raw material is better, and the water absorption rate will slightly decrease with the increase of the dosage of isocyanate.

[0115] It can also be seen from Examples 1 and 12-15 that the preferred usage ratio of prepolymer, crosslinker TMP and polysiloxane is 1:(0.2-0.3):(0.3-0.5). Within this range, the crosslinking modification effect is better, and beyond this range, the performance decreases. Analysis shows that this may be related to steric hindrance.

[0116] It can also be seen from Examples 1 and 16-20 that when the polysiloxane is composed of hydroxyl-terminated polydimethylsiloxane, carbon hydroxyl-terminated polydimethylsiloxane and N-(β-aminoethyl)-γ-aminopropyltrimethoxysilane, the modified crosslinking effect is optimal;

[0117] The preferred weight ratio of the three is 1:(1-2):(0.5-0.8), and the reasons may be as follows:

[0118] Carbon hydroxyl-modified polydimethylsiloxane, N-(β-aminoethyl)-γ-aminopropyltrimethoxysilane and terminal hydroxyl polydimethylsiloxane undergo more complete multiple cross-linking reactions with the polyurethane component, and the hydrophobicity, scratch resistance and adhesion of the copolymer can be significantly improved through further reaction of the active carbon hydroxyl groups in the copolymer with the active groups in the polyurethane.

[0119] This specific application example is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the application example without any creative contribution as needed. However, as long as it is within the scope of the claims of the present application, it shall be protected by the patent law.

Claims

1. A water-based polymer coating for a wiper blade, characterized in that: It is composed of the following components in parts by weight: 40-60 parts of modified waterborne polyurethane dispersion, 3-5 parts of dispersant, 8-12 parts of solid lubricant, 8-10 parts of polydimethylsiloxane, 0.9-1.8 parts of functional additives, and 18-22 parts of deionized water; The synthetic method of the modified aqueous polyurethane resin dispersion is as follows: S1. Prepolymer synthesis: polycarbonate diol, excess isophorone diisocyanate and catalyst DBTDL are prepolymerized in a DMF solution at a dosage ratio of 1:(2.4-3.6):(0.005-0.008) at 50-60° C. for 10-15 h under a nitrogen atmosphere, and dried to obtain a prepolymer; S2, cross-linking modification: adding a cross-linking agent TMP and polysiloxane to the prepolymer, wherein the amount ratio of the prepolymer, the cross-linking agent TMP and the polysiloxane is 1:(0.2-0.3):(0.3-0.5), reacting at 70-80° C. for 40-56 hours under a nitrogen atmosphere, to obtain a modified waterborne polyurethane resin dispersion; The polysiloxane is composed of hydroxyl-terminated polydimethylsiloxane, carbon hydroxyl-terminated polydimethylsiloxane and N-(β-aminoethyl)-γ-aminopropyltrimethoxysilane in a weight ratio of 1:(1-2):(0.5-0.8); The solid lubricant is selected from one or more of molybdenum disulfide, graphite and boron nitride.

2. The water-based polymer coating for a wiper blade according to claim 1, characterized in that: The functional additive consists of a wetting agent, a leveling agent and a defoaming agent.

3. The method for using the water-based polymer coating for a wiper blade according to claim 1 or 2, characterized in that: The specific steps are as follows: Weigh each component of the coating in proportion, mix and stir until fully uniform, spray it on both sides of the wiper blade edge, and then cure it at 100-120℃ for 5-15 minutes and then cool it.

4. Application of the water-based polymer coating for wiper blades according to claim 1 or 2, characterized in that: For wiper blades made of neoprene.

Citation Information

Patent Citations

  • Preparation method for organosilicon-modified crosslinking polyurethane emulsion

    CN103382245A

  • Waterborne polyurethane environment-friendly coating for automobile windshield wiper rubber strip and preparation method thereof

    CN112409907A