A multi-scale endogenously reinforced magnesium-based amorphous composite material and a preparation method thereof

CN116288075BActive Publication Date: 2024-11-26HUAZHONG UNIV OF SCI & TECH +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310435086.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-04-21
Publication Date
2024-11-26
Estimated Expiration
2043-04-21

AI Technical Summary

Technical Problem

In existing magnesium-based amorphous composite materials, the volume fraction of the reinforced phase is low and the morphology and size is difficult to regulate, resulting in less obvious improvement in strength and plasticity, high preparation and smelting temperature and high cost.

Method used

Multi-scale endogenous reinforced magnesium-based amorphous composite material is used, and the composition expression is (Mg0.65Cu0.075Ni0.075Ag0.05Zn0.05Gd0.05)100-xFex, where 5≤x≤30, the matrix is ​​Mg-Cu-Ni -Ag-Zn-Gd-Y amorphous alloy, the reinforced phase is porous Fe particles, and the selective elements of Ni-Fe solid solution prealloy powder and Mg-Cu-(Ni)-Ag-Zn-Gd-Y metal melt are passed through the selective elements of Ni-Fe solid solution pre-alloy powder and Mg-Cu-(Ni)-Ag-Zn-Gd-Y metal melt. Dissolve to form a porous reinforced phase, which is dispersed in the matrix.

Benefits of technology

The fracture strength and room temperature plasticity of magnesium-based amorphous composite materials are significantly improved, and the volume fraction of the reinforced phase is 9% to 19%. The average size and ligament size of porous Fe particles are adjustable, achieving efficient and energy-saving production and improving the material. mechanical properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116288075B_ABST
    Figure CN116288075B_ABST
Patent Text Reader

Abstract

The present invention belongs to the technical field of magnesium-based amorphous composite materials, and more specifically, relates to a multi-scale endogenously reinforced magnesium-based amorphous composite material and a preparation method thereof. The composition expression of the composite material is (Mg 0.65 Cu 0.075 Ni 0.075 Ag 0.05 Zn 0.05 G 0.05 Y 0.05 ) 100‑ x Fe x , wherein x represents the atomic ratio, and 5≤x≤30; the matrix of the composite material is Mg‑Cu‑Ni‑Ag‑Zn‑Gd‑Y amorphous alloy; the reinforcing phase is endogenous porous Fe particles, and the reinforcing phase is dispersed in the matrix. The present invention introduces the reinforcing phase through Ni‑Fe solid solution pre-alloying, and can prepare a magnesium-based amorphous composite material with high fracture strength, large plastic deformation, high volume fraction of the reinforcing phase, and stable morphology and size. The process is simple, the melting temperature for preparing the magnesium-based amorphous composite material is low, the cost is low, and efficient and energy-saving production can be achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the field of magnesium-based amorphous composite materials, and more specifically, relates to a multi-scale endogenously reinforced magnesium-based amorphous composite material and a preparation method thereof. Background Art

[0002] Thanks to its unique "short-range order and long-range disorder" structure, magnesium-based amorphous alloys have the advantages of high strength, high elastic limit, corrosion resistance and other performance advantages, and are a kind of structural material with great potential. However, during the deformation process at room temperature, magnesium-based amorphous alloys show the characteristics of room temperature brittleness due to the formation of highly localized shear bands, which limits their wide application. At present, the room temperature plasticity of magnesium-based amorphous alloys can be improved by introducing a reinforcing phase to prepare magnesium-based amorphous composites. The methods of introducing reinforcing phases are mainly divided into two types: direct addition method and in-situ self-generation method. However, the bonding strength between the second phase obtained by the direct addition method and the amorphous matrix is ​​low, resulting in no obvious improvement in the mechanical properties of the composite material; while in the in-situ self-generation method, the bonding strength between the reinforcement and the amorphous matrix is ​​high, but its preparation process is difficult to design. Patent document CN103451577A discloses a quasi-crystal particle reinforced magnesium-based amorphous alloy endogenous composite material and a preparation method thereof, wherein the method for preparing the quasi-crystal-amorphous endogenous composite structure is simple, easy to operate and highly controllable; Patent document CN114672744A discloses an endogenous porous titanium reinforced magnesium-based amorphous composite material and a preparation method thereof, wherein the reinforcing phase size of the invention can reach the submicron level, which can significantly increase the plasticity of the material; Patent document CN101348889A discloses an iron particle reinforced magnesium-based amorphous alloy composite material and a preparation method thereof, wherein the method overcomes the problem of brittle fracture of amorphous alloys and improves the plasticity of the material by directly adding iron particles of different volume fractions.

[0003] However, the interface bonding between the reinforcing phase and the matrix introduced into magnesium-based amorphous composites by the direct addition method is poor, and the effect on improving the plasticity of the material is limited; the reinforcing phase introduced into magnesium-based amorphous composites by the existing in-situ self-generation method often has problems such as difficulty in controlling the morphology and size, low volume fraction of the reinforcing phase, and no obvious improvement in material plasticity. The melting temperature of the synthesized magnesium-based amorphous composites is high, and the cost is high. Summary of the invention

[0004] In view of the defects of the prior art, the purpose of the present invention is to provide a multi-scale endogenously reinforced magnesium-based amorphous composite material and a preparation method thereof, so as to solve the problems of low volume fraction of the reinforcing phase in the existing magnesium-based amorphous composite materials, difficult to control the morphology and size, no obvious improvement in the strength and plasticity of the magnesium-based amorphous composite materials, high melting temperature and high preparation cost in the preparation of magnesium-based amorphous composite materials.

[0005] To achieve the above object, the present invention provides a multi-scale endogenously reinforced magnesium-based amorphous composite material, the composition expression of the composite material is (Mg0.65 Cu 0.075 Ni 0.075 Ag 0.05 Zn 0.05 G 0.05 Y 0.05 ) 100-x Fe x , where x represents the atomic ratio, and 5≤x≤30;

[0006] The matrix of the composite material is Mg-Cu-Ni-Ag-Zn-Gd-Y amorphous alloy; the reinforcing phase in the composite material is porous Fe particles, and the porous Fe particles are dispersed in the matrix.

[0007] Preferably, the average size of the porous Fe particles is 20 μm to 80 μm, and the average size of the ligaments is 0.5 μm to 8 μm.

[0008] The present invention also provides a method for preparing a multi-scale endogenously reinforced magnesium-based amorphous composite material, comprising the following steps:

[0009] S1, mixing and smelting Cu, Ni, Gd, and Y raw materials, and obtaining a Cu-Ni-Gd-Y pre-alloy ingot after cooling; mixing Ni and Fe raw materials, performing vacuum melting and atomization treatment, and obtaining a Ni-Fe solid solution pre-alloy powder;

[0010] S2, mixing and smelting the Cu-Ni-Gd-Y pre-alloy ingot with Mg, Ag, and Zn raw materials, adding the Ni-Fe solid solution pre-alloy powder after fully melting, stirring at the same temperature, and obtaining a master alloy ingot after cooling;

[0011] S3. Vacuum-melting the master alloy ingot to obtain the multi-scale endogenously reinforced magnesium-based amorphous composite material.

[0012] Preferably, in steps S1 and S2, the atomic ratio of the Cu, Ni, Gd, Y, Fe, Mg, Ag, and Zn raw materials satisfies the expression (Mg 0.65 Cu 0.075 Ni 0.075 Ag 0.05 Zn 0.05 G 0.05 Y 0.05 ) 100-x Fe x , where 5≤X≤30.

[0013] Preferably, in step S1, the particle size of the Ni—Fe solid solution pre-alloyed powder is 20 μm to 100 μm, and the atomic ratio of Ni / Fe in the Ni—Fe solid solution pre-alloyed powder is 0.3 to 3.

[0014] Preferably, in steps S1, S2 and S3, the vacuum degree of the smelting is independently 2×10 -3 Pa~6×10 - 3 Pa, the protective gas is an inert gas with a purity of 99.999%, and the atmospheric pressure of the protective gas is independently -0.02 MPa to -0.06 MPa.

[0015] Preferably, in step S1, the mixed smelting is vacuum arc melting, and the temperature of the vacuum arc melting is 1800°C to 2400°C; the melting temperature for preparing the Ni-Fe solid solution pre-alloyed powder is 1800°C to 2400°C, and during the atomization process, the atomizing gas is an inert gas with a purity of 99.999%, and the pressure of the atomizing gas is 1MPa to 3MPa.

[0016] Preferably, in step S2, the mixed smelting is vacuum induction smelting, the smelting temperature for preparing the master alloy ingot is 600°C to 750°C, the insulation stirring time is 1 min to 6 min, and the stirring speed is 300 to 1200 r / min.

[0017] Preferably, in step S3, the vacuum melting is vacuum induction melting, preferably, the vacuum induction melting is spray casting melting, and the spray casting melting is specifically: cutting the prepared master alloy ingot into pieces and placing it in a crucible with a small hole at the bottom, then evacuating the vacuum and introducing a protective gas, then induction heating the master alloy ingot, applying an inert gas of a preset pressure to the melt after it is completely melted, so as to spray the melt into a mold below the crucible, and obtaining the multi-scale endogenously reinforced magnesium-based amorphous composite material after cooling.

[0018] Preferably, the atmosphere pressure of the inert gas is -0.03 MPa to -0.06 MPa, and the preset pressure of the inert gas is 0.01 MPa to 0.06 MPa.

[0019] In general, the above technical solution conceived by the present invention has the following advantages compared with the prior art:

[0020] Beneficial effects:

[0021] (1) The present invention provides a multi-scale endogenously reinforced magnesium-based amorphous composite material, wherein the matrix of the composite material is a Mg-Cu-Ni-Ag-Zn-Gd-Y amorphous alloy, which has a high amorphous forming ability and is easy to form an amorphous matrix; the reinforcing phase of the composite material is porous Fe particles, and the porous Fe particles are dispersed in the above-mentioned matrix. The composite material provided by the present application has the advantages of high fracture strength, large plastic deformation, and high volume fraction of the reinforcing phase. Specifically, the multi-scale endogenously reinforced magnesium-based amorphous composite material provided by the present invention has a fracture strength increased by 3.9% to 21.2% compared with the matrix alloy, a plastic deformation of 4.2% to 11.7%, and a volume fraction of the reinforcing phase of 9% to 19%.

[0022] (2) In the multi-scale intrinsically reinforced magnesium-based amorphous composite material provided by the present invention, the average size of the porous Fe particles is tens of microns, the average size of the ligaments is submicron, and the particle configuration of tens of microns and the submicron ligament structure constitute a multi-scale reinforcement structure between and inside the particles, forming a three-dimensional continuous network locally in the matrix, so that the bonding strength between the reinforcement phase (porous Fe particles) and the matrix is ​​high, thereby ensuring that the composite material has better mechanical properties, and the fracture strength and room temperature plasticity are significantly improved.

[0023] (3) The present invention is based on the principle of selective element dissolution. By mixing Ni-Fe solid solution pre-alloy powder with Mg-Cu-(Ni)-Ag-Zn-Gd-Y metal melt, the Ni element is selectively dissolved in the Mg-Cu-(Ni)-Ag-Zn-Gd-Y metal melt, and the remaining Fe element is aggregated by surface diffusion to form a porous reinforcement phase, which is dispersed in the matrix. The difference in Young's modulus between the reinforcement phase and the matrix leads to stress concentration at the interface, thereby inhibiting the rapid expansion of a single shear band, causing shear band proliferation, and improving the plastic deformation capacity of the composite material. Compared with the existing preparation method, the present invention can adjust the Ni-Fe solid solution pre-alloy particle size, Ni / Fe ratio, temperature, time and stirring rate of selective element dissolution to achieve adjustable and controllable pore morphology, porosity and pore size of the reinforcement phase in the magnesium-based amorphous composite material, thereby preparing a magnesium-based amorphous composite material with higher strength and greater plastic deformation. In addition, the activation energy required for the selective element dissolution of the Ni-Fe solid solution pre-alloy and the melt in the present invention is only 120 kJ / mol, which is lower than that of other systems. Therefore, the Ni-Fe solid solution phase can achieve complete selective element dissolution at a lower temperature and in a shorter time, thereby achieving efficient and energy-saving production.

[0024] (4) The present invention introduces the reinforcement phase through Ni-Fe solid solution pre-alloy. Compared with the introduction of the reinforcement phase through compound pre-alloy, first, the Ni-Fe solid solution pre-alloy used in the present invention is a single-phase FCC structure, which will not undergo complex phase changes during selective element dissolution, and the generated porous reinforcement phase has stable morphology and size and uniform structure; second, the Ni-Fe solid solution phase has uniform structure and a wide adjustable range of the ratio of the two elements, so that the pore structure of the porous reinforcement phase generated in the magnesium-based amorphous composite material has a wide adjustable range, and further, the pore size of the generated porous reinforcement phase can be regulated in a wider range; third, the present invention can also achieve a large volume content of powder addition by reducing the Ni content, thereby increasing the volume content of the reinforcement phase. Specifically, the average size of the reinforcement phase (porous Fe particles) in a multi-scale endogenously reinforced magnesium-based amorphous composite material provided by the present invention is 20μm to 80μm, the ligament size is 0.5μm to 8μm, the porosity is 30% to 70%, and the volume fraction is 9% to 19%.

[0025] (5) The present invention designs the smelting process according to the characteristics of each raw material, including the vacuum degree, smelting temperature, smelting time, protective gas purity, protective gas atmosphere pressure, protective gas preset pressure, etc. during the smelting process, so that the fracture strength of the magnesium-based amorphous composite material prepared by the present invention is significantly improved, and it has good plastic deformation ability. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 is a preparation flow chart of a multi-scale endogenously reinforced magnesium-based amorphous composite material provided by an embodiment of the present invention;

[0027] Figure 2 In Example 1 (Mg 0.65 Cu 0.075 Ni 0.075 Ag 0.05 Zn 0.05 G 0.05 Y 0.05 ) 70 Fe 30 Scanning electron microscope image of magnesium-based amorphous composites;

[0028] Figure 3 In Example 1 (Mg 0.65 Cu 0.075 Ni 0.075 Ag 0.05 Zn 0.05 G 0.05 Y 0.05 ) 70 Fe 30An equiaxial compressive stress-strain curve of a magnesium-based amorphous composite material and a shear band generated during the compression of the composite material, wherein content (a) is an equiaxial compressive stress-strain curve of the magnesium-based amorphous composite material; content (b) is a shear band generated during the compression of the magnesium-based amorphous composite material;

[0029] Figure 4 is a scanning electron microscope image of the reinforcement phase in the magnesium-based amorphous composite material prepared in Examples 1 and 2, wherein content (a) is the (Mg 0.65 Cu 0.075 Ni 0.075 Ag 0.05 Zn 0.05 G 0.05 Y 0.05 ) 70 Fe 30 SEM image of porous reinforcement phase in magnesium-based amorphous composite material, content (b) is the (Mg 0.65 Cu 0.075 Ni 0.075 Ag 0.05 Zn 0.05 G 0.05 Y 0.05 ) 75 Fe 25 Scanning electron microscope image of porous reinforcement phase in magnesium-based amorphous composites;

[0030] Figure 5 In Comparative Example 2 (Mg 0.65 Cu 0.075 Ni 0.075 Ag 0.05 Zn 0.05 G 0.05 Y 0.05 ) 60 Fe 40 Morphology of the master alloy ingot. DETAILED DESCRIPTION

[0031] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention.

[0032] The present invention provides a multi-scale endogenously reinforced magnesium-based amorphous composite material, the composition expression of which is (Mg 0.65 Cu 0.075 Ni 0.075 Ag 0.05 Zn 0.05 G 0.05 Y 0.05 ) 100-x Fex , wherein x represents the atomic ratio, and 5≤x≤30; the matrix of the composite material is Mg-Cu-Ni-Ag-Zn-Gd-Y amorphous alloy; the reinforcing phase in the composite material is porous Fe particles, and the porous Fe particles are dispersed in the matrix.

[0033] In some embodiments, the average size of the porous Fe particles is 20 μm to 80 μm, the average size of the ligaments is 0.5 μm to 8 μm, the porosity is 30% to 70%, and the volume fraction is 9% to 19%.

[0034] The matrix of the composite material of the present invention is a Mg-Cu-Ni-Ag-Zn-Gd-Y amorphous alloy, which has high amorphous forming ability and is easy to form an amorphous matrix; the reinforcing phase of the composite material is porous Fe particles, the macroscopic size of the porous Fe particles reaches tens of microns, the ligament size reaches submicron level, and the particle configuration of tens of microns and the submicron ligament structure constitute a multi-scale reinforcement structure between and inside the particles, forming a three-dimensional continuous network locally in the matrix, thereby ensuring that the composite material has better mechanical properties, and the fracture strength and room temperature plasticity are significantly improved.

[0035] like Figure 1 As shown, the present invention provides a method for preparing a multi-scale endogenously reinforced magnesium-based amorphous composite material, the method comprising the following steps:

[0036] S1, Cu, Ni, Gd and Y raw materials are mixed and smelted, and after cooling, a Cu-Ni-Gd-Y pre-alloy ingot is obtained; Ni and Fe raw materials are mixed and vacuum smelted and atomized to obtain Ni-Fe solid solution pre-alloy powder;

[0037] S2, mixing and smelting the Cu-Ni-Gd-Y pre-alloy ingot with Mg, Ag, and Zn raw materials, adding the Ni-Fe solid solution pre-alloy powder after fully melting, stirring at the same temperature, and obtaining a master alloy ingot after cooling;

[0038] S3. Vacuum-melting the master alloy ingot to obtain the multi-scale endogenously reinforced magnesium-based amorphous composite material.

[0039] The present invention is based on the principle of selective element dissolution. The Ni-Fe solid solution pre-alloy powder is mixed with a Mg-Cu-(Ni)-Ag-Zn-Gd-Y metal melt, wherein the Ni element is selectively dissolved in the Mg-Cu-(Ni)-Ag-Zn-Gd-Y metal melt, and the remaining Fe element is aggregated by surface diffusion to form a porous reinforcement phase, which is dispersed in the matrix. Specifically, the difference in Young's modulus between the porous reinforcement phase and the matrix leads to stress concentration at the interface, thereby inhibiting the rapid expansion of a single shear band, causing shear band proliferation, and improving the plastic deformation capacity of the magnesium-based amorphous composite material. Compared with the existing preparation methods, the present invention can control the size, volume fraction, morphology and porosity of the reinforcement phase over a wide range, thereby preparing a magnesium-based amorphous composite material with higher fracture strength and greater plastic deformation; at the same time, the activation energy required for the selective element dissolution of the Ni-Fe solid solution pre-alloy and the melt in the present invention is only 120 kJ / mol, which is lower than that of other systems. Therefore, the Ni-Fe solid solution phase can achieve complete selective element dissolution at a lower temperature and in a shorter time, thereby achieving efficient and energy-saving production.

[0040] In some embodiments, step S1 specifically includes the following steps:

[0041] Ingredients:

[0042] According to the atomic fraction ratio satisfying the expression (Mg 0.65 Cu 0.075 Ni 0.075 Ag 0.05 Zn 0.05 G 0.05 Y 0.05 ) 100-x Fe x , where 5≤X≤30, the raw materials Cu, Zn, Gd, Y, Fe, Mg, Ag and Ni-Fe solid solution pre-alloyed powder are prepared.

[0043] In some embodiments, the raw materials of copper bars, nickel particles, gadolinium blocks, yttrium blocks, iron particles, magnesium blocks, silver particles, and zinc particles are polished to remove surface oxide scale, ultrasonically cleaned in anhydrous ethanol and dried to ensure the high purity of each raw material. Preferably, the purity of the copper bars, nickel particles, gadolinium blocks, yttrium blocks, iron particles, magnesium blocks, silver particles, and zinc particles used in the embodiments of the present invention is greater than 99.9%.

[0044] In some embodiments, the particle size of the Ni-Fe solid solution pre-alloyed powder is 20 to 100 μm. This is because if the particle size is too small, the Ni-Fe solid solution pre-alloyed powder will agglomerate, while if the particle size is too large, the reinforcing phase ligaments will be coarse, weakening the reinforcing effect. In some embodiments, the atomic ratio of Ni / Fe in the Ni-Fe solid solution pre-alloyed powder is 0.3 to 3. If the ratio is too small, it will be difficult to form a fully open porous Fe reinforced structure. If the ratio is too large, the porosity of the porous structure will be too high after the selective element dissolution, causing the particles to collapse and break.

[0045] Based on the particle size of the above-mentioned Ni-Fe solid solution pre-alloyed powder and the atomic ratio of Ni / Fe, in some embodiments of the present invention, the range of x is 5≤x≤30, preferably, 10≤x≤30. The inventors found through experiments that when x is 2.5, the content of the reinforcing phase introduced into the composite material is small, and it is difficult to significantly improve the plasticity of the composite material; when x is 40, the addition amount of Ni-Fe solid solution pre-alloyed powder in the metal melt is too high, and a large amount of Ni-Fe solid solution pre-alloyed powder is difficult to enter the melt through stirring, and finally agglomerates and bonds to the surface of the master alloy ingot, resulting in deviations in the matrix composition of the magnesium-based amorphous composite material.

[0046] Preparation of Cu-Ni-Gd-Y pre-alloyed ingot:

[0047] The configured copper bars, nickel particles, gadolinium blocks, and yttrium blocks are mixed and smelted to obtain a Cu-Ni-Gd-Y pre-alloyed ingot. The present invention does not limit the method of the above-mentioned mixed smelting. In some embodiments, the above-mentioned mixed smelting is vacuum arc smelting. Specifically, the above-mentioned configured alloy raw materials are placed in a vacuum arc melting furnace, evacuated and a protective gas is introduced, and the alloy raw materials are arc-smelted. After sufficient smelting, the Cu-Ni-Gd-Y pre-alloyed ingot is obtained by cooling.

[0048] In some embodiments, the vacuum degree of arc melting is 3×10 -3 Pa~5×10 -3 Pa, the protective gas used is an inert gas with a purity of 99.999%, and the atmosphere pressure of the protective gas is -0.02MPa to -0.06MPa, which can effectively protect the alloy from oxidation, and effectively avoid the evaporation of the raw material alloy while ensuring that the raw material alloy is fully melted, thereby ensuring the performance of the alloy. The arc melting temperature is 1800℃ to 2400℃, and the alloy raw materials need to be melted multiple times, preferably more than 3 times. Each time the alloy raw materials are melted, they need to be kept for a period of time, and they need to be turned over between each two meltings to ensure that the structure and composition of the alloy ingots are uniform.

[0049] Preparation of Ni-Fe solid solution pre-alloyed powder:

[0050] The configured Ni and Fe raw materials are vacuum melted and atomized to obtain Ni-Fe solid solution pre-alloyed powder. The present invention does not limit the above-mentioned vacuum melting method. In some embodiments, the above-mentioned vacuum melting is vacuum arc melting. In some embodiments, the melting temperature for preparing the Ni-Fe solid solution pre-alloyed powder is 1800°C to 2400°C. During the atomization process, the atomizing gas is an inert gas with a purity of 99.999%, and the pressure of the atomizing gas is 1MPa to 3MPa. The present invention can achieve precise control of the size, volume fraction, and porosity of the reinforcing phase by controlling the Ni / Fe ratio and particle size.

[0051] In some embodiments, step S2 specifically includes the following steps:

[0052] Preparation of master alloy ingot:

[0053] The Cu-Ni-Gd-Y pre-alloyed ingot is mixed with Mg, Ag, and Zn raw materials for smelting, and after being fully melted, the Ni-Fe solid solution pre-alloyed powder is added, and the mixture is kept warm and stirred, and then cooled to obtain a master alloy ingot. Specifically, the Cu-Ni-Gd-Y pre-alloyed ingot is cut into small pieces, and placed in a high-purity graphite crucible with magnesium blocks, silver particles, and zinc particles. The Ni-Fe solid solution pre-alloyed powder is placed in a powder adding tank, and a protective gas is introduced after vacuuming to perform induction heating smelting. After being fully melted, the Ni-Fe solid solution pre-alloyed powder is added to the melt, and the mixture is kept warm and stirred, so that the Ni-Fe solid solution pre-alloyed powder and the melt undergo selective element dissolution to obtain a semi-solid melt. Finally, the semi-solid melt is poured into a mold, and then cooled to obtain a master alloy ingot.

[0054] In some embodiments, the vacuum degree during melting is 3×10 -3 Pa~5×10 -3 Pa, the protective gas is an inert gas with a purity of 99.999%, and the atmosphere pressure of the protective gas is -0.02MPa~-0.06Mpa.

[0055] The present invention designs the smelting conditions according to the melting points and other characteristics of each raw material metal block and alloy block. Cu, Ni, Gd, and Y have relatively high melting points. If they are induction-melted together with Mg, Ag, and Zn, the raw materials cannot be fully melted and mixed evenly, which leads to uneven alloy composition and requires arc melting. Mg, Ag, and Zn have relatively low boiling points. When arc-melted together with Cu, Ni, Gd, and Y, they are easily evaporated and gasified. Therefore, arc melting is first used to melt Cu, Ni, Gd, and Y to obtain a Cu-Ni-Gd-Y pre-alloy with uniform alloy composition, and then mixed with Mg, Ag, and Zn for induction melting. At the same time, the protective gas during the smelting process can effectively prevent the metal raw materials from being oxidized during the smelting process.

[0056] Furthermore, in step S2 of the present invention, the Ni-Fe solid solution pre-alloy powder is used to introduce the reinforcement phase, and the size and pore size of the reinforcement phase can be regulated by the solid solution characteristics and the preparation process, that is, the reaction kinetics can be changed by regulating the reaction parameters. In some embodiments, in step S2, the smelting temperature for preparing the master alloy ingot is 600℃~750℃, and the insulation time is 1min~6min. If the smelting time is too long or the smelting temperature is too high, the reinforcement phase ligaments will diffuse and grow under the temperature drive, weakening the reinforcement effect; if the smelting time is too short or the smelting temperature is too low, the selective elements will not be fully dissolved, and it will be difficult to form a dispersed and small-sized reinforcement phase. In some embodiments, the mechanical stirring speed is 300~1200r / min. If the speed is too low, it will be difficult to fully stir the melt, and the powder particles will partially melt and bond, reducing the dispersion effect. If the speed is too high, the solid solution powder will be thrown out, resulting in a reduction in the introduction of the reinforcement phase and a deviation in the matrix composition of the magnesium-based amorphous composite material.

[0057] In some embodiments, step S3 specifically includes the following steps:

[0058] Preparation of magnesium-based amorphous composite materials:

[0059] The master alloy ingot is vacuum melted to obtain a multi-scale endogenously reinforced magnesium-based amorphous composite material. In some embodiments, the magnesium-based amorphous composite material is prepared by vacuum induction melting; preferably, the vacuum induction melting is spray casting melting.

[0060] In some embodiments, the specific operation of the above-mentioned spray casting and melting is: cutting the above-mentioned master alloy ingot into blocks and placing it in a quartz tube with a small hole at the bottom, then evacuating the tube and introducing a protective gas, then induction heating the master alloy ingot, applying an inert gas with a preset pressure to the melt after it is completely melted, so as to spray the melt into a mold under the crucible, and obtaining a multi-scale endogenously reinforced magnesium-based amorphous composite material after cooling.

[0061] In some embodiments, the vacuum degree of the spray casting is 3×10 -3 Pa~5×10 -3 Pa, the protective gas used is an inert gas with a purity of 99.999%, and the atmosphere pressure of the inert gas is -0.02MPa~-0.06Mpa, that is, the furnace chamber pressure is -0.02MPa~-0.06Mpa. During the spray casting and smelting process, if the furnace chamber pressure is too low, the protective atmosphere will be insufficient and the raw material smelting process will be unstable. If the furnace chamber pressure is too high, the atmospheric pressure in the environment will reduce the pressing effect of the furnace door, thereby causing air leakage in the smelting furnace and affecting the accuracy of the composition of the magnesium-based amorphous composite material.

[0062] In some embodiments, the diameter of the small hole at the bottom of the quartz tube crucible is 1.1 mm to 1.5 mm. If the diameter of the small hole at the bottom of the quartz tube crucible is too large, the melt after smelting may fall directly through the small hole; if the diameter is too small, the melt is not easy to be ejected.

[0063] In some embodiments, the preset pressure of the inert gas is 0.01MPa to 0.06MPa, so that the melt can fully enter the copper mold before cooling and solidification, so that it is completely filled, and at the same time, the melt is prevented from being drawn into the gas, thereby ensuring that no porosity defects will be generated in the sample after solidification. Preferably, the above-mentioned mold is a copper mold with an inner diameter of 2mm to 5mm. Selecting copper molds of different sizes and shapes can control the cooling rate of the melt and the shape of the obtained magnesium-based amorphous composite material.

[0064] The invention is based on the principle of selective element dissolution, and the Ni-Fe solid solution pre-alloy powder is mixed with a Mg-Cu-(Ni)-Ag-Zn-Gd-Y metal melt, wherein the Ni element is selectively dissolved in the Mg-Cu-(Ni)-Ag-Zn-Gd-Y metal melt, and the remaining Fe element is aggregated by surface diffusion to form a porous reinforcement phase, which is dispersed in the matrix. The matrix of the magnesium-based amorphous composite material prepared by the invention is a Mg-Cu-Ni-Ag-Zn-Gd-Y amorphous alloy, which has a high amorphous forming ability and is easy to form an amorphous matrix; the reinforcement phase of the magnesium-based amorphous composite material is porous Fe particles, the macroscopic size of the porous Fe particles reaches tens of microns, and the ligament size reaches submicron level, wherein the particle configuration of tens of microns and the submicron ligament structure constitute a multi-scale reinforcement structure between particles and inside particles, and form a three-dimensional continuous network locally in the matrix, which can ensure that the magnesium-based amorphous composite material has better mechanical properties, and the fracture strength and room temperature plasticity are significantly improved.

[0065] The present invention can adjust the Ni-Fe solid solution pre-alloy particle size, Ni / Fe ratio, temperature, time and stirring rate of selective element dissolution to achieve adjustable and controllable pore morphology, porosity and pore size of the reinforcement phase in the magnesium-based amorphous composite material, thereby preparing a magnesium-based amorphous composite material with higher strength and greater plastic deformation. In addition, the activation energy required for the selective element dissolution of the Ni-Fe solid solution pre-alloy and the melt in the present invention is only 120kJ / mol, which is less than other systems. Therefore, the Ni-Fe solid solution phase can achieve complete selective element dissolution at a lower temperature and in a shorter time, thereby achieving efficient and energy-saving production. In a preferred embodiment of the present invention, the smelting temperature for preparing the master alloy ingot is 600°C to 750°C, and the insulation time is 1min to 6min. The multi-scale endogenously enhanced magnesium-based amorphous composite material finally obtained has a fracture strength increased by 3.9% to 21.2% compared to the matrix alloy, and the plastic deformation is 4.2% to 11.7%.

[0066] The above technical solution is described in detail below in conjunction with specific embodiments:

[0067] Example 1

[0068] 1) Grind copper bars, nickel particles, gadolinium blocks, yttrium blocks, iron particles, magnesium blocks, silver particles, and zinc particles with a purity of 99.9% to remove surface oxide scale, then perform ultrasonic cleaning in anhydrous ethanol, dry, and then perform the following steps: 0.65 Cu 0.075 Ni 0.07 5Ag 0.05 Zn 0.05 G 0.05 Y 0.05 ) 70 Fe 30 The atomic formula is used to prepare copper bars, nickel particles, gadolinium blocks, yttrium blocks, iron particles, magnesium blocks, silver particles, and zinc particles.

[0069] 2) Place the prepared copper bars, nickel particles, gadolinium blocks and yttrium blocks into a vacuum arc melting furnace and evacuate to 4×10 -3 Pa, argon gas is introduced into the vacuum chamber until the chamber pressure is -0.05MPa; the raw materials are arc-melted at a melting temperature of 1900-2200°C, the alloy ingot is kept for 3 minutes after being completely melted, and then the alloy ingot is turned over by a turning rod and re-melted, each alloy ingot is melted 4 times in total, and after the melting is completed, it is cooled on a water-cooled copper mold, and the Cu-Ni-Gd-Y pre-alloyed ingot is taken out; the nickel particles and iron particles are prepared into Ni-Fe pre-alloyed ingots using the above method, wherein Ni / Fe=0.8, and Ni-Fe solid solution pre-alloyed powder with a particle size of 20-70μm is screened out after atomization powder making.

[0070] 3) Cut the Cu-Ni-Gd-Y pre-alloy into appropriate small pieces and place them in a graphite crucible together with magnesium blocks, silver particles and zinc particles. Place the Ni-Fe solid solution pre-alloy powder in a powder adding tank and evacuate to 3×10 -3 Pa, argon gas is introduced into the vacuum chamber until the chamber pressure is -0.05MPa; the metal is induction heated and melted, and Ni-Fe solid solution pre-alloy powder is added after it is fully melted. The mechanical stirring head is inserted into the melt and stirring is started. The speed is set to 1000r / min, and selective element dissolution is carried out at 700℃. Stirring is stopped after 3 minutes, and then the semi-solid melt is poured into the copper mold below. The induction current is turned off, and after cooling to room temperature, the (Mg 0.65 Cu 0.075 Ni 0.075 Ag 0.05 Zn 0.05 G 0.05 Y 0.05 ) 70 Fe 30 Master alloy ingot.

[0071] 4) Cut the master alloy ingot into appropriate small pieces and put them into a quartz tube with a bottom hole diameter of 1.5 mm, and evacuate to 4×10 - 3 After the molten alloy is melted, argon gas is introduced into the vacuum chamber until the chamber pressure is -0.06MPa. The induction heating is turned on and the induction current is slowly adjusted until the alloy block is completely melted. An argon gas flow with a pressure of 0.04MPa is sprayed from above the melt to spray the melt into a copper mold with a diameter of 5mm. The induction current is turned off and the melt is cooled to room temperature. A 5mm (Mg 0.65 Cu 0.075 Ni 0.075 Ag 0.05 Zn 0.05 G 0.05 Y 0.05 ) 70 Fe 30 Magnesium-based amorphous composites.

[0072] Figure 2 is (Mg 0.65 Cu 0.075 Ni 0.075 Ag 0.05 Zn 0.05 G 0.05 Y 0.05 ) 70 Fe 30 The scanning electron microscope image of magnesium-based amorphous composite material shows that (Mg 0.65 Cu 0.075 Ni 0.075 Ag 0.05 Zn 0.05 G 0.05 Y 0.05 ) 70 Fe 30 The magnesium-based amorphous composite material is mainly composed of a magnesium-based amorphous matrix and a porous reinforcement phase α-Fe. When the Ni-Fe solid solution pre-alloyed powder is added to the melt, selective element dissolution occurs, the Ni in the solid solution pre-alloyed powder reacts with the Mg, Ag and other elements in the melt and dissolves into it, while the Fe element gradually accumulates to form a three-dimensional continuous porous structure through diffusion migration, and the generated porous Fe is dispersed in the Mg-Cu-Ni-Ag-Zn-Gd-Y amorphous matrix.

[0073] Figure 3 Content (a) is (Mg 0.65 Cu 0.075 Ni 0.075 Ag 0.05 Zn 0.05 G 0.05 Y 0.05 ) 70 Fe 30True stress-strain curve of magnesium-based amorphous composites under equiaxial compression test, which shows that in the equiaxial compression test, (Mg 0.65 Cu 0.075 Ni 0.075 Ag 0.05 Zn 0.05 G 0.05 Y 0.05 ) 70 Fe 30 The amorphous alloy with the following composition enters plastic deformation after elastic deformation and eventually breaks, with a fracture strength of 1087MPa; while the fracture strength of the pure amorphous matrix is ​​897MPa, with no obvious plasticity. (Mg 0.65 Cu 0.075 Ni 0.075 Ag 0.05 Zn 0.05 G 0.05 Y 0.05 ) 70 Fe 30 The fracture strength of the magnesium-based amorphous composite material is increased by 21.2% compared with the matrix alloy, and the most critical room temperature plasticity is also significantly improved. The plastic deformation of the magnesium-based amorphous composite material prepared in this embodiment is as high as 11.7%. Figure 3 Content (b) is (Mg 0.65 Cu 0.075 Ni 0.075 Ag 0.05 Zn 0.05 G 0.05 Y 0.05 ) 70 Fe 30 The shear bands produced during the compression deformation of magnesium-based amorphous composites show that the introduction of a large number of reinforcing phases promotes the proliferation and offset of the shear bands, inhibits the rapid expansion of the shear bands, and improves the strength and plasticity of the magnesium-based amorphous composites.

[0074] The generated porous Fe has uniform size, an average size of 45 μm, a volume fraction of 19%, and a porosity of 45%. Figure 4 Content (a) is (Mg 0.65 Cu 0.075 Ni 0.075 Ag 0.05 Zn 0.05 G 0.05 Y 0.05 ) 70 Fe 30Scanning electron microscope image of porous reinforcing phase α-Fe in magnesium-based amorphous composite materials. The image shows that the generated porous Fe ligaments are uniform in size, with an average ligament size of 5μm. The reinforcing phase interface is tightly bonded to the matrix, and the matrix composition inside the reinforcing phase pores is uniform and stable. Macroscopic particles of tens of microns and submicron ligament structures constitute a multi-scale reinforcing phase structure between and within particles, forming a three-dimensional continuous network locally in the matrix, which significantly enhances the comprehensive performance of magnesium-based amorphous composites.

[0075] Example 2

[0076] 1) Grind copper bars, nickel particles, gadolinium blocks, yttrium blocks, iron particles, magnesium blocks, silver particles, and zinc particles with a purity of 99.9% to remove surface oxide scale, then perform ultrasonic cleaning in anhydrous ethanol, dry, and then perform the following steps: 0.65 Cu 0.075 Ni 0.07 5Ag 0.05 Zn 0.05 G 0.05 Y 0.05 ) 75 Fe 25 The atomic formula is used to prepare copper bars, nickel particles, gadolinium blocks, yttrium blocks, iron particles, magnesium blocks, silver particles, and zinc particles.

[0077] 2) Place the prepared copper bars, nickel particles, gadolinium blocks and yttrium blocks into a vacuum arc melting furnace and evacuate to 4×10 -3 Pa, argon gas is introduced into the vacuum chamber until the chamber pressure is -0.06MPa; the raw materials are arc-melted at a melting temperature of 1900-2200°C, the alloy ingot is kept for 3 minutes after being completely melted, and then the alloy ingot is turned over by a turning rod and re-melted, each alloy ingot is melted 4 times in total, and after the melting is completed, it is cooled on a water-cooled copper mold, and the Cu-Ni-Gd-Y pre-alloyed ingot is taken out; the nickel particles and iron particles are prepared into Ni-Fe pre-alloyed ingots using the above method, wherein Ni / Fe=3, and Ni-Fe solid solution pre-alloyed powder with a particle size of 30-60μm is screened out after atomization powder making.

[0078] 3) Cut the Cu-Ni-Gd-Y pre-alloy into appropriate small pieces and place them in a graphite crucible together with magnesium blocks, silver particles and zinc particles. Place the Ni-Fe solid solution pre-alloy powder in a powder adding tank and evacuate to 4×10 -3 Pa, argon gas is introduced into the vacuum chamber until the chamber pressure is -0.06MPa; the metal is induction heated and melted, and Ni-Fe solid solution pre-alloy powder is added after it is fully melted. The mechanical stirring head is inserted into the melt and stirring is started. The speed is set to 1200r / min, and selective element dissolution is carried out at 750℃. Stirring is stopped after 1min, and then the semi-solid melt is poured into the copper mold below. The induction current is turned off, and after cooling to room temperature, the (Mg 0.65 Cu0.075 Ni 0.075 Ag 0.05 Zn 0.05 G 0.05 Y 0.05 ) 75 Fe 25 Master alloy ingot.

[0079] 4) Cut the master alloy ingot into appropriate small pieces and put them into a quartz tube with a bottom hole diameter of 1.1 mm, and evacuate to 4×10 - 3 After the molten alloy is melted, argon gas is introduced into the vacuum chamber until the chamber pressure is -0.06MPa. The induction heating is turned on and the induction current is slowly adjusted until the alloy block is completely melted. An argon gas flow with a pressure of 0.04MPa is sprayed from above the melt to spray the melt into a copper mold with a diameter of 3mm. The induction current is turned off and the melt is cooled to room temperature. A 3mm (Mg 0.65 Cu 0.075 Ni 0.075 Ag 0.05 Zn 0.05 G 0.05 Y 0.05 ) 75 Fe 25 Magnesium-based amorphous composites.

[0080] In the equiaxial compression test, (Mg 0.65 Cu 0.075 Ni 0.075 Ag 0.05 Zn 0.05 G 0.05 Y 0.05 ) 75 Fe 25 The amorphous alloy with the composition enters plastic deformation after elastic deformation and finally breaks. The fracture strength is 1053MPa, which is 17.4% higher than that of the matrix alloy, and the plastic deformation is as high as 9.6%.

[0081] The generated porous Fe has uniform size, an average size of 50 μm, a volume fraction of 15%, and a porosity of 70%. Figure 4 Content (b) is (Mg 0.65 Cu 0.075 Ni 0.075 Ag 0.05 Zn 0.05 G 0.05 Y 0.05 ) 75 Fe 25Scanning electron microscope image of the porous reinforcing phase α-Fe in the magnesium-based amorphous composite material. The image shows that the generated porous Fe ligaments are uniform in size, with an average ligament size of 8μm, the interface of the reinforcing phase is tightly bonded to the matrix, and the matrix composition inside the pores of the reinforcing phase is uniform and stable.

[0082] Example 3

[0083] 1) Grind copper bars, nickel particles, gadolinium blocks, yttrium blocks, iron particles, magnesium blocks, silver particles, and zinc particles with a purity of 99.9% to remove surface oxide scale, then perform ultrasonic cleaning in anhydrous ethanol, dry, and then perform the following steps: 0.65 Cu 0.075 Ni 0.07 5Ag 0.05 Zn 0.05 G 0.05 Y 0.05 ) 80 Fe 20 The atomic formula is used to prepare copper bars, nickel particles, gadolinium blocks, yttrium blocks, iron particles, magnesium blocks, silver particles, and zinc particles.

[0084] 2) Place the prepared copper bars, nickel particles, gadolinium blocks and yttrium blocks into a vacuum arc melting furnace and evacuate to 3×10 -3 Pa, argon gas is introduced into the vacuum chamber until the chamber pressure is -0.04MPa; the raw materials are arc-melted at a melting temperature of 1900-2100°C, the alloy ingot is kept for 3 minutes after being completely melted, and then the alloy ingot is turned over by a turning rod and re-melted, each alloy ingot is melted 4 times in total, and after the melting is completed, it is cooled on a water-cooled copper mold, and the Cu-Ni-Gd-Y pre-alloyed ingot is taken out; the nickel particles and iron particles are prepared into Ni-Fe pre-alloyed ingots using the above method, wherein Ni / Fe=2, and Ni-Fe solid solution pre-alloyed powder with a particle size of 50-100μm is screened out after atomization powder making.

[0085] 3) Cut the Cu-Ni-Gd-Y pre-alloy into appropriate small pieces and place them in a graphite crucible together with magnesium blocks, silver particles and zinc particles. Place the Ni-Fe solid solution pre-alloy powder in a powder adding tank and evacuate to 3×10 -3 Pa, argon gas was introduced into the vacuum chamber until the chamber pressure was -0.04MPa; the metal was induction heated and melted, and Ni-Fe solid solution pre-alloy powder was added after it was fully melted. The mechanical stirring head was inserted into the melt and began to stir. The speed was set to 800r / min, and the selective element dissolution was carried out at 680℃. The stirring was stopped after 4 minutes, and then the semi-solid melt was poured into the copper mold below. The induction current was turned off, and after cooling to room temperature, the (Mg 0.65 Cu 0.075 Ni 0.075 Ag 0.05 Zn 0.05 G 0.05Y 0.05 ) 80 Fe 20 Master alloy ingot.

[0086] 4) Cut the master alloy ingot into appropriate small pieces and put them into a quartz tube with a bottom hole diameter of 1.1 mm, and evacuate to 3×10 - 3 After the molten alloy is melted, argon gas is introduced into the vacuum chamber until the chamber pressure is -0.04 MPa. The induction heating is turned on and the induction current is slowly adjusted until the alloy block is completely melted. An argon gas flow with a pressure of 0.06 MPa is sprayed from above the melt to spray the melt into a copper mold with a diameter of 3 mm. The induction current is turned off and the melt is cooled to room temperature. A 3 mm (Mg 0.65 Cu 0.075 Ni 0.075 Ag 0.05 Zn 0.05 G 0.05 Y 0.05 ) 80 Fe 20 Magnesium-based amorphous composites.

[0087] The generated porous Fe has uniform size, with an average size of 70 μm, an average ligament size of 8 μm, a volume fraction of 12%, a porosity of 60%, a close bond between the reinforcement phase interface and the matrix, and a uniform and stable matrix composition inside the reinforcement phase pores.

[0088] In the equiaxial compression test, (Mg 0.65 Cu 0.075 Ni 0.075 Ag 0.05 Zn 0.05 G 0.05 Y 0.05 ) 80 Fe 20 The amorphous alloy with the composition enters plastic deformation after elastic deformation and finally breaks. The fracture strength is 1013MPa, which is 12.9% higher than that of the matrix alloy, and the plastic deformation is as high as 7.5%.

[0089] Example 4

[0090] 1) Grind copper bars, nickel particles, gadolinium blocks, yttrium blocks, iron particles, magnesium blocks, silver particles, and zinc particles with a purity of 99.9% to remove surface oxide scale, then perform ultrasonic cleaning in anhydrous ethanol, dry, and then perform the following steps: 0.65 Cu 0.075 Ni 0.07 5Ag 0.05 Zn 0.05 G 0.05 Y 0.05 ) 85 Fe15 The atomic formula is used to prepare copper bars, nickel particles, gadolinium blocks, yttrium blocks, iron particles, magnesium blocks, silver particles, and zinc particles.

[0091] 2) Place the prepared copper bars, nickel particles, gadolinium blocks and yttrium blocks into a vacuum arc melting furnace and evacuate to 3×10 -3 Pa, argon gas is passed into the vacuum chamber until the chamber pressure is -0.05MPa, the raw materials are arc melted, the melting temperature is 2000-2200°C, the alloy ingot is kept for 3 minutes after being completely melted, and then the alloy ingot is turned over by a turning rod and re-melted, each alloy ingot is melted 4 times in total, and after the melting is completed, it is cooled on a water-cooled copper mold, and the Cu-Gd-Ni-Y pre-alloyed ingot is taken out; the nickel particles and iron particles are prepared into Ni-Fe pre-alloyed ingots using the above method, wherein Ni / Fe=0.5, and Ni-Fe solid solution pre-alloyed powder with a particle size of 30-80μm is screened out after atomization powder making.

[0092] 3) Cut the Cu-Ni-Gd-Y pre-alloy into appropriate small pieces and place them in a graphite crucible together with magnesium blocks, silver particles and zinc particles. Place the Ni-Fe solid solution pre-alloy powder in a powder adding tank and evacuate to 3×10 -3 Pa, argon gas is introduced into the vacuum chamber until the chamber pressure is -0.05MPa; the metal is induction heated and melted, and Ni-Fe solid solution pre-alloy powder is added after it is fully melted. The mechanical stirring head is inserted into the melt and stirring is started. The speed is set to 500r / min, and selective element dissolution is carried out at 650℃. Stirring is stopped after 6 minutes, and then the semi-solid melt is poured into the copper mold below. The induction current is turned off, and after cooling to room temperature, the (Mg 0.65 Cu 0.075 Ni 0.075 Ag 0.05 Zn 0.05 G 0.05 Y 0.05 ) 85 Fe 15 Master alloy ingot.

[0093] 4) Cut the master alloy ingot into appropriate small pieces and put them into a quartz tube with a bottom hole diameter of 1.4 mm, and evacuate to 3×10 - 3 After the molten alloy is melted, argon gas is introduced into the vacuum chamber until the chamber pressure is -0.05MPa. The induction heating is turned on and the induction current is slowly adjusted until the alloy block is completely melted. An argon gas flow with a pressure of 0.02MPa is sprayed from above the melt to spray the melt into a copper mold with a diameter of 2mm. The induction current is turned off and the melt is cooled to room temperature. A 2mm (Mg 0.65 Cu 0.075 Ni 0.075 Ag 0.05 Zn 0.05 G0.05 Y 0.05 ) 85 Fe 15 Magnesium-based amorphous composite material; the generated porous Fe is dispersed in the Mg-Cu-Ni-Ag-Zn-Gd-Y amorphous matrix, the porous Fe has a uniform size, an average size of 50 μm, an average ligament size of 4 μm, a volume fraction of 9%, and a porosity of 30%.

[0094] In the equiaxial compression test, (Mg 0.65 Cu 0.075 Ni 0.075 Ag 0.05 Zn 0.05 G 0.05 Y 0.05 ) 85 Fe 15 The amorphous alloy with the composition enters plastic deformation after elastic deformation and finally breaks with a fracture strength of 932MPa. Compared with the base alloy, the fracture strength increases by 3.9% and the plastic deformation reaches 4.2%.

[0095] Comparative Example 1

[0096] 1) Grind copper bars, nickel particles, gadolinium blocks, yttrium blocks, iron particles, magnesium blocks, silver particles, and zinc particles with a purity of 99.9% to remove surface oxide scale, then perform ultrasonic cleaning in anhydrous ethanol, dry, and then perform the following steps: 0.65 Cu 0.075 Ni 0.07 5Ag 0.05 Zn 0.05 G 0.05 Y 0.05 ) 97.5 Fe 2.5 The atomic formula is used to prepare copper bars, nickel particles, gadolinium blocks, yttrium blocks, iron particles, magnesium blocks, silver particles, and zinc particles.

[0097] 2) Place the prepared copper bars, nickel particles, gadolinium blocks and yttrium blocks into a vacuum arc melting furnace and evacuate to 5×10 -3 Pa, argon gas is introduced into the vacuum chamber until the chamber pressure is -0.06MPa; the raw materials are arc-melted at a melting temperature of 1800-2400°C, the alloy ingot is kept for 3 minutes after being completely melted, and then the alloy ingot is turned over by a turning rod and re-melted, the alloy ingot is melted 4 times in total, and after the melting is completed, it is cooled on a water-cooled copper mold, and the Cu-Ni-Gd-Y pre-alloyed ingot is taken out; the nickel particles and iron particles are prepared into Ni-Fe pre-alloyed ingots using the above method, wherein Ni / Fe=1, and Ni-Fe solid solution pre-alloyed powder with a particle size of 15-30μm is screened out after atomization powder making.

[0098] 3) Cut the Cu-Ni-Gd-Y pre-alloy into appropriate small pieces and place them in a graphite crucible together with magnesium blocks, silver particles and zinc particles. Place the Ni-Fe solid solution pre-alloy powder in a powder adding tank and evacuate to 3×10 -3 Pa, argon gas was introduced into the vacuum chamber until the chamber pressure was -0.04MPa; the metal was induction heated and melted, and Ni-Fe solid solution pre-alloy powder was added after it was fully melted. The mechanical stirring head was inserted into the melt and began to stir. The speed was set to 900r / min, and the selective element was dissolved at 600℃. The stirring was stopped after 7min, and then the semi-solid melt was poured into the copper mold below. The induction current was turned off, and after cooling to room temperature, the (Mg 0.65 Cu 0.075 Ni 0.075 Ag 0.05 Zn 0.05 G 0.05 Y 0.05 ) 97.5 Fe 2.5 Master alloy ingot.

[0099] 4) Cut the master alloy ingot into suitable small pieces and put them into a quartz tube with a bottom hole diameter of 1 mm, and evacuate to 3×10 -3 After the molten alloy is melted, argon gas is introduced into the vacuum chamber until the chamber pressure is -0.05 MPa. The induction heating is turned on and the induction current is slowly adjusted until the alloy block is completely melted. An argon gas flow with a pressure of 0.015 MPa is sprayed from above the melt and the melt is sprayed into a copper mold with a diameter of 2 mm. The induction current is turned off and the melt is cooled to room temperature. A 2 mm (Mg 0.65 Cu 0.075 Ni 0.075 Ag 0.05 Zn 0.05 G 0.05 Y 0.05 ) 97.5 Fe 2.5 Magnesium-based amorphous composite material; the average size of porous Fe is 23μm, the average size of ligament is 3μm, its fracture strength is 923MPa, and the plastic deformation is 0.4%. Due to the small content of the introduced reinforcement phase, it is difficult to significantly improve the plasticity of magnesium-based amorphous composite materials.

[0100] Comparative Example 2

[0101] 1) Grind copper bars, nickel particles, gadolinium blocks, yttrium blocks, iron particles, magnesium blocks, silver particles, and zinc particles with a purity of 99.9% to remove surface oxide scale, then perform ultrasonic cleaning in anhydrous ethanol, dry, and then perform the following steps: 0.65 Cu 0.075 Ni 0.07 5Ag 0.05 Zn 0.05 G0.05 Y 0.05 ) 60 Fe 40 The atomic formula is used to prepare copper bars, nickel particles, gadolinium blocks, yttrium blocks, iron particles, magnesium blocks, silver particles, and zinc particles.

[0102] 2) Place the prepared copper bars, nickel particles, gadolinium blocks and yttrium blocks into a vacuum arc melting furnace and evacuate to 5×10 -3 Pa, argon gas is introduced into the vacuum chamber until the chamber pressure is -0.06MPa; the raw materials are arc-melted at a melting temperature of 1800-2400°C, the alloy ingot is kept for 3 minutes after being completely melted, and then the alloy ingot is turned over by a turning rod and re-melted, the alloy ingot is melted 4 times in total, and after the melting is completed, it is cooled on a water-cooled copper mold, and the Cu-Ni-Gd-Y pre-alloyed ingot is taken out; the nickel particles and iron particles are prepared into Ni-Fe pre-alloyed ingots using the above method, wherein Ni / Fe=1, and Ni-Fe solid solution pre-alloyed powder with a particle size of 20-50μm is screened out after atomization powder making.

[0103] 3) Cut the Cu-Ni-Gd-Y pre-alloy into appropriate small pieces and place them in a graphite crucible together with magnesium blocks, silver particles and zinc particles. Place the Ni-Fe solid solution pre-alloy powder in a powder adding tank and evacuate to 3×10 -3 Pa, argon gas is introduced into the vacuum chamber until the chamber pressure is -0.04MPa; the metal is induction heated and melted, and Ni-Fe solid solution pre-alloy powder is added after it is fully melted. The mechanical stirring head is inserted into the melt and stirring is started. The speed is set to 1200r / min, and selective element dissolution is carried out at 750℃. Stirring is stopped after 7min, and then the semi-solid melt is poured into the copper mold below. The induction current is turned off, and after cooling to room temperature, the (Mg 0.65 Cu 0.075 Ni 0.075 Ag 0.05 Zn 0.05 G 0.05 Y 0.05 ) 60 Fe 40 Master alloy ingot.

[0104] 4)(Mg 0.65 Cu 0.075 Ni 0.075 Ag 0.05 Zn 0.05 G 0.05 Y 0.05 ) 60 Fe 40 The morphology of the master alloy ingot is as follows Figure 5As shown, it can be seen that there is a layer of agglomerated powder on the surface of the master alloy ingot. This is because the Ni-Fe solid solution pre-alloy powder is added in too much amount, and it is still difficult to completely enter the melt after sufficient stirring, and finally agglomerates and bonds to the surface of the master alloy ingot. The composition analysis found that the Fe atomic ratio in the master alloy ingot is only 23%, indicating that the matrix composition of the composite material prepared in this comparative example deviates from that of the target composite material.

[0105] It will be easily understood by those skilled in the art that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A multi-scale endogenously reinforced magnesium-based amorphous composite material, characterized in that: The composition expression of the composite material is (Mg 0.65 Cu 0.075 Ni 0.075 Ag 0.05 Zn 0.05 G 0.05 Y 0.05 ) 100-x Fe x , where x represents the atomic ratio, and 5≤x≤30; The matrix of the composite material is Mg-Cu-Ni-Ag-Zn-Gd-Y amorphous alloy; the reinforcing phase in the composite material is porous Fe particles, the average size of the porous Fe particles is 20 μm to 80 μm, the average size of the ligaments is 0.5 μm to 8 μm, and the porous Fe particles are dispersed in the matrix; The method for preparing the multi-scale endogenously reinforced magnesium-based amorphous composite material comprises the following steps: S1, mixing and smelting Cu, Ni, Gd, and Y raw materials, and obtaining a Cu-Ni-Gd-Y pre-alloy ingot after cooling; mixing Ni and Fe raw materials, performing vacuum melting and atomization treatment, and obtaining a Ni-Fe solid solution pre-alloy powder; The particle size of the Ni-Fe solid solution pre-alloyed powder is 20 μm to 100 μm, and the atomic ratio of Ni / Fe in the Ni-Fe solid solution pre-alloyed powder is 0.3 to 3; S2, mixing and smelting the Cu-Ni-Gd-Y pre-alloy ingot with Mg, Ag, and Zn raw materials, adding the Ni-Fe solid solution pre-alloy powder after fully melting, stirring at the same temperature, and obtaining a master alloy ingot after cooling; The mixed smelting is vacuum induction smelting, the smelting temperature of the obtained master alloy ingot is 600°C to 750°C, the insulation stirring time is 1min to 6min, and the stirring speed is 300 to 1200r / min; S3. Vacuum-melting the master alloy ingot to obtain the multi-scale endogenously reinforced magnesium-based amorphous composite material.

2. The multi-scale endogenously reinforced magnesium-based amorphous composite material according to claim 1, characterized in that: In steps S1, S2 and S3, the vacuum degree of the smelting is independently 2×10 -3 Pa~6×10 -3 Pa, the protective gas is an inert gas with a purity of 99.999%, and the atmosphere pressure of the protective gas is independently -0.02MPa~-0.06MPa.

3. The multi-scale endogenously reinforced magnesium-based amorphous composite material according to claim 1, characterized in that: In step S1, the mixed smelting is vacuum arc melting, and the temperature of the vacuum arc melting is 1800°C~2400°C; the melting temperature of the obtained Ni-Fe solid solution pre-alloyed powder is 1800°C~2400°C, and during the atomization process, the atomizing gas is an inert gas with a purity of 99.999%, and the pressure of the atomizing gas is 1MPa~3MPa.

4. The multi-scale endogenously reinforced magnesium-based amorphous composite material according to claim 1, characterized in that: In step S3, the vacuum melting is vacuum induction melting.

5. The multi-scale endogenously reinforced magnesium-based amorphous composite material according to claim 4, characterized in that: The vacuum induction melting is spray casting melting, and the spray casting melting is specifically as follows: the prepared master alloy ingot is cut into pieces and placed in a crucible with a small hole at the bottom, and then vacuum is evacuated and a protective gas is introduced, and then the master alloy ingot is induction heated, and after it is completely melted, an inert gas with a preset pressure is applied to the melt to spray the melt into a mold below the crucible, and after cooling, the multi-scale endogenously reinforced magnesium-based amorphous composite material is obtained.

6. The multi-scale endogenously reinforced magnesium-based amorphous composite material according to claim 5, characterized in that: The atmosphere pressure of the inert gas is -0.03MPa~-0.06Mpa, and the preset pressure of the inert gas is 0.01MPa~0.06MPa.