The iron-based amorphous soft magnetic alloy powder composed of elements was prepared and optimized by aerosolization method. Combined with special treatment, the problem of insufficient amorphous formation ability and coercivity in the existing technology was solved, and a high-frequency magnetic powder core was realized , improves performance and scope of application.
Patent Information
- Application Number
- CN202310584681.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-23
- Publication Date
- 2024-11-26
AI Technical Summary
The amorphous formation ability and coercivity of the existing iron-based amorphous soft magnetic alloys are insufficient, making it difficult to meet the low loss and high efficiency requirements of high-frequency electronic components. In addition, traditional preparation methods have a long time, easy pollution and poor spherical shape. The problem.
The iron-based amorphous soft magnetic alloy powder was prepared by aerosolization method. By controlling the atomic percentage of elements such as P, C, B, Si, Mo, Cr and V, it was prepared with high amorphous formation ability and low correction. An alloy with stubborn force and excellent soft magnetic properties combines phosphating, coupling and insulation treatment to prepare a high-frequency and suitable magnetic powder core.
The high amorphous formation ability and low coercive force of iron-based amorphous soft magnetic alloy is realized, and the critical size of the magnetic powder core is improved to the millimeter level. The saturation magnetization and induction strength are significantly improved, and the loss is less than 800kW/m3, and the effective magnetic conductance is effective. The rate is greater than 20 and is suitable for high-frequency inductance and electronic communication fields.
Smart Images

Figure CN119028688A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of soft magnetic material preparation, and specifically relates to an iron-based amorphous soft magnetic alloy and a preparation method and application thereof. Background Art
[0002] Amorphous alloys are different from traditional crystalline metals in that their microstructure is disordered in the long range but ordered in the short range. As a new generation of soft magnetic materials, iron-based amorphous alloys have the advantages of high saturation magnetic induction and low coercivity. Soft magnetic amorphous alloy ribbons have been widely used in the cores of transformers, inductors, mutual inductors and other devices.
[0003] Recently, researchers have turned their attention to the field of soft magnetic composite powder cores. After adding a binder to Fe-based amorphous powder and molding it under certain conditions, the soft magnetic composite powder core can achieve miniaturization and complex application of devices. Compared with pure iron or silicon steel, Fe-based amorphous alloys have lower coercivity and higher resistivity, and the prepared magnetic powder core has low loss, which improves efficiency and frequency of use. Compared with ferrites, etc., Fe-based amorphous alloys have higher saturation magnetic induction intensity, and the size of the device is smaller under the same working magnetic induction. The soft magnetic composite powder core made of Fe-based amorphous powder has excellent comprehensive soft magnetic properties, and its advantages of low loss, high efficiency and high power density at high frequencies are more obvious, making it have broad prospects in the fields of electronic communications, one-piece molded inductor components, etc.
[0004] The preparation of Fe-based amorphous soft magnetic alloy powder and its use in the manufacture of magnetic powder cores are still in the initial stage, with low saturation magnetization intensity, which cannot meet the higher requirements of technological development. In addition, amorphous forming ability is also an important indicator of the soft magnetic properties of Fe-based amorphous soft magnetic alloys. Fe-based amorphous alloy powders are usually prepared by gas atomization, water atomization, and mechanical crushing and ball milling. Among them, the ball milling method has problems such as long time consumption, easy pollution, and sharp surface angles that are not conducive to high-frequency applications, and is not suitable for high-frequency electronic components. Compared with gas atomization, water atomization has a higher cooling rate, but the sphericity of the prepared powder shape is not good. The powder prepared by gas atomization has good sphericity and high quality, but the alloy component needs to have very high forming ability and powdering ability. At present, most alloy component systems are prepared by water atomization or water-gas combined atomization, and amorphous structure can only be obtained when the powder size is small (usually less than 20-30μm), but the sphericity and quality of gas atomized amorphous powder are better than those of water atomization. Therefore, the preparation of iron-based soft magnetic amorphous alloy powder by gas atomization and water atomization still needs to increase research and development efforts, especially the alloy components that can be used to prepare amorphous alloy powder by gas atomization can often also be used to prepare amorphous alloy powder by water atomization. Therefore, it is more important and more challenging to develop an iron-based amorphous alloy component system that can be used to prepare amorphous alloy powder by gas atomization.
[0005] For amorphous soft magnetic alloys, in addition to the amorphous forming ability of the alloy, the coercivity of the amorphous alloy is an important soft magnetic property index. Among the amorphous alloys developed so far, there are few iron-based amorphous alloy systems with a coercivity less than 2 A / m, and amorphous alloys with a coercivity less than 1 A / m are very rare. Reducing the coercivity of amorphous soft magnetic alloys is very important for reducing losses. Therefore, it is necessary to develop amorphous alloy compositions and amorphous alloy powder materials with high amorphous forming ability, low coercivity, and excellent soft magnetic properties, and to study the preparation of amorphous alloy powders and magnetic powder cores with low losses at high frequencies. Summary of the Invention
[0006] Therefore, the technical problem to be solved by the present invention is how to develop an amorphous alloy composition with high amorphous forming ability, low coercivity, and high soft magnetic properties, thereby providing an iron-based amorphous soft magnetic alloy, its preparation method, and application.
[0007] To this end, the present invention provides the following technical solutions.
[0008] The present invention provides an iron-based amorphous soft magnetic alloy having the general formula shown in Formula I,
[0009] Fe (100-a-b-c-d-e-f) P a C b B c Si d Mo e N f , Formula I
[0010] Wherein, a, b, c, d, e, and f respectively represent the atomic percentages of P, C, B, Si, Mo, and N. Based on 100% of the atomic percentage, a% + b% + c% + d% + e% + f% = 100%; the value ranges of a, b, c, d, e, and f are 3 ≤ a ≤ 8, 4 ≤ b ≤ 12, 5 ≤ c ≤ 11, 2.8 ≤ d ≤ 3.2, 0 ≤ e ≤ 5, and 0 ≤ e + f ≤ 5;
[0011] N is at least one of Cr and V.
[0012] In the iron-based amorphous soft magnetic alloy, when 4 ≤ b ≤ 6, f < 1;
[0013] When 6 < b ≤ 12, 0 ≤ f ≤ 2.
[0014] The iron-based amorphous soft magnetic alloy is an alloy block, alloy strip, or alloy powder.
[0015] When the iron-based amorphous soft magnetic alloy is an alloy strip, before use, it needs to be annealed, and the annealing temperature is (T x -100) °C to (T x -200) °C; wherein, T xis the crystallization temperature.
[0016] The present invention also provides a method for preparing an iron-based amorphous soft magnetic alloy powder, wherein the components of the iron-based amorphous soft magnetic alloy powder are selected from the above-mentioned iron-based amorphous soft magnetic alloy, and the preparation method comprises the following steps:
[0017] Ingredients:
[0018] Smelting to obtain a master alloy ingot;
[0019] The master alloy ingot is melted, atomized by gas atomization, and solidified to obtain the iron-based amorphous soft magnetic alloy powder. During the atomization, the atmosphere can be nitrogen or argon.
[0020] The present invention also provides a method for preparing a magnetic powder core, wherein the iron-based amorphous soft magnetic alloy powder prepared by the above-mentioned preparation method comprises the following steps:
[0021] The iron-based amorphous soft magnetic alloy powder is subjected to phosphating, coupling and insulation treatments in sequence, and then is subjected to cold pressing and heat treatment.
[0022] The preparation method comprises using a phosphating liquid to phosphate the powder;
[0023] Preferably, the phosphating treatment time is 30-60 minutes and the temperature is 40-60°C;
[0024] Preferably, the phosphating solution is a phosphoric acid solution.
[0025] The preparation method uses a silane coupling agent to perform the coupling; preferably, the coupling time is 5-10 minutes and the temperature is 40-60°C;
[0026] Preferably, the insulation treatment is performed using silicone resin, epoxy resin or polytetrafluoroethylene.
[0027] The cold pressing pressure is 500-2000MPa and the time is 5-10min;
[0028] Preferably, the specific steps of the heat treatment include keeping the temperature in a protective atmosphere at 300-500° C. for at least 1 hour;
[0029] Preferably, the protective atmosphere is at least one of argon and nitrogen.
[0030] The invention also provides a magnetic powder core obtained by the preparation method.
[0031] In addition, the present invention also provides a magnetic powder core obtained by the above preparation method or the application of the above magnetic powder core in the fields of high-frequency inductance, high-frequency switching power supply or electronic communication.
[0032] The technical solution of the present invention has the following advantages:
[0033] 1. The iron-based amorphous soft magnetic alloy provided by the present invention has the general formula Fe (100-a-b-c-d-e-f) P a C b B c Si d Mo e N f The iron-based amorphous soft magnetic alloy provided by the present invention can have high amorphous forming ability, low coercive force and excellent soft magnetic properties, and the critical size of the iron-based amorphous soft magnetic alloy can be improved to the millimeter level. The prior art has extremely high requirements on the amorphous forming ability when preparing materials mainly based on iron-based amorphous powder. The critical size of the iron-based amorphous soft magnetic alloy prepared by the present invention can reach the millimeter level, which further illustrates that the amorphous forming ability of the iron-based amorphous soft magnetic alloy provided by the present invention is excellent. The iron-based amorphous soft magnetic alloy provided by the present invention has excellent soft magnetic properties. The iron-based amorphous soft magnetic alloy block or iron-based amorphous soft magnetic alloy strip has an induction intensity B under an external field of 800A / m. 800 ≥1.0T, saturation magnetization M s The best can reach 1.50T, the coercive force H c Can be as low as 0.6A / m; the saturation magnetization intensity M of iron-based amorphous soft magnetic alloy powder under 800kA / m external field s >110emu / g.
[0034] The present invention controls the atomic percentage of each element in the iron-based amorphous soft magnetic alloy, and by controlling the percentage of the iron element, the soft magnetic alloy can be ensured to have a critical size of the millimeter level; there is a synergistic effect between the various elements in the iron-based amorphous soft magnetic alloy, which can ensure the amorphous forming ability and soft magnetic properties of the alloy. Based on research and theoretical analysis, the present invention adopts low silicon, utilizes the interaction and synergy between the P, C, and B elements, and their influence on the amorphous forming ability and soft magnetic properties, and then determines the iron-based amorphous soft magnetic alloy proposed by the present invention, which can have high amorphous forming ability, low coercive force and high soft magnetic properties.
[0035] The invention adds Mo to the iron-based amorphous soft magnetic alloy, which helps to further increase the critical size to the millimeter level and make the soft magnetic alloy into amorphous powder; adding Cr and / or V helps to improve the amorphous forming ability, and the Cr element helps to improve the corrosion resistance of the iron-based amorphous, is not easily contaminated in the subsequent process, and is beneficial to improving the magnetic properties of the alloy. Controlling the addition amount of Mo, Cr and / or V in the range of 0-5% can not only ensure that the alloy has high amorphous forming ability, but also keep the soft magnetic properties of the alloy at a high level, and achieve a balance between the amorphous alloy forming ability and the soft magnetic properties.
[0036] 2. The preparation method of the iron-based amorphous soft magnetic alloy provided by the present invention can prepare amorphous alloy powder by a gas atomization method. The powder is spherical, and there is no obvious crystallization peak in the X-ray diffraction spectrum of the powder after the impurities are screened out, and the powder has a completely amorphous structure.
[0037] 3. The magnetic powder core provided by the present invention has a loss of less than 800kW / m when tested under 100kHz and 100mT conditions. 3 , the effective magnetic permeability is greater than 20, and can be stabilized to 10 6 Hz; DC bias capability is greater than 80% at 100Oe. BRIEF DESCRIPTION OF THE DRAWINGS
[0038] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0039] Figure 1 is the X-ray diffraction pattern of the alloy rods prepared in various embodiments of the present invention;
[0040] Figure 2 The X-ray diffraction patterns of the unscreened powder and five grades of powders prepared by gas atomization of the alloy powder obtained in Example 1 of the present invention;
[0041] Figure 3 is a scanning electron microscope photograph of the alloy powder of Example 1 of the present invention;
[0042] Figure 4 1 is the DSC curve of the alloy powders prepared in Example 1 and Example 2 of the present invention;
[0043] Figure 5 is the hysteresis loop of the alloy powders prepared in Example 1 and Example 2 of the present invention;
[0044] Figure 6 The X-ray diffraction patterns of the unscreened powder and five grades of powders prepared by gas atomization of the alloy powder obtained in Example 2 of the present invention;
[0045] Figure 7 is a scanning electron microscope photograph of the alloy powder of Example 2 of the present invention;
[0046] Figure 8 These are the X-ray diffraction patterns of three grades of alloy powder of Comparative Example 1 of the present invention. DETAILED DESCRIPTION
[0047] The following examples are provided for a better understanding of the present invention, but are not intended to limit the best mode of implementation, nor to limit the content and protection scope of the present invention. Any product identical or similar to the present invention obtained by anyone under the inspiration of the present invention or by combining the features of the present invention with other prior arts shall fall within the protection scope of the present invention.
[0048] If no specific experimental steps or conditions are specified in the examples, the conventional experimental steps or conditions described in the literature in the field can be used. If no manufacturer is specified for the reagents or instruments used, they are all conventional reagent products that can be obtained commercially.
[0049] Example 1
[0050] This embodiment provides an iron-based amorphous soft magnetic alloy having the general formula Fe 73 P8C7B6Si3Mo3;
[0051] This embodiment also provides a method for preparing an iron-based amorphous soft magnetic alloy rod having a general formula of Fe 73 P8C7B6Si3Mo3, comprising the following steps:
[0052] Fe, Mo, Si with a purity greater than 99.5wt.% and FeC, FeB, FeP with a purity greater than 99wt.% are prepared according to a general formula to obtain a raw material mixture. An induction melting furnace is used, the cavity is evacuated and filled with argon gas, and the raw material mixture is repeatedly melted 4 times to ensure uniform composition, and a master alloy ingot is obtained for standby use.
[0053] The master alloy ingot is placed in a quartz crucible with a nozzle, heated to above the melting point, and when the alloy is completely melted, 0.05MPa argon is filled into the quartz crucible, and the melt is sprayed into a copper mold with an inner hole size of at least Ф1mm to obtain an alloy rod.
[0054] The cross section of the alloy rod was examined by X-ray diffractometer, such as Figure 1 As shown, there is no obvious crystallization peak under the distinguishable conditions in the spectrum, indicating that the prepared alloy rod has an amorphous structure and is a rod-shaped bulk amorphous alloy material, that is, the alloy has a rod-shaped critical size (referred to as critical size) for forming an amorphous structure of more than 1 mm. The critical size of the iron-based amorphous soft magnetic alloy rod prepared in this embodiment is shown in Table 2.
[0055] This embodiment also provides a method for preparing an iron-based amorphous soft magnetic alloy strip having a general formula of Fe 73 P8C7B6Si3Mo3, comprising the following steps:
[0056] The method for preparing the master alloy ingot is the same as above.
[0057] The master alloy ingot is placed in a quartz crucible with a nozzle, heated to above the melting point, and when the alloy is completely melted, 0.05MPa argon gas is injected into the quartz crucible, and the melt is sprayed onto the surface of a copper roller with a rotation speed of 35m / s, and cooled to obtain an amorphous alloy strip. The soft magnetic properties of the amorphous alloy strip are tested by annealing the amorphous alloy strip at 370℃ and testing it under an external field of 800kA / m. The saturation magnetization intensity M of the amorphous alloy strip is s It is 1.21T, tested under an external field of 800A / m, the magnetic induction intensity B 800 1.19T, coercive force H c It is about 0.9A / m. The specific results are shown in Table 2.
[0058] This embodiment also provides a method for preparing an iron-based amorphous soft magnetic alloy powder having a general formula of Fe 73 P8C7B6Si3Mo3, comprising the following steps:
[0059] The method for preparing the master alloy ingot is the same as above.
[0060] The master alloy ingot is placed in a crucible in a gas atomization furnace and heated to above the melting point. After the alloy is completely melted, it is atomized under the action of high-pressure argon gas, and after cooling and solidification, fine spherical powder is formed, i.e., amorphous alloy spherical powder; wherein, those skilled in the art can determine the atomization pressure according to the equipment and the melting conditions of the alloy liquid. The amorphous alloy spherical powder is graded using a standard sieve to obtain five levels of powders, i.e., -50-+200 mesh, -200-+300 mesh, -300-+500 mesh, -500-+800 mesh and -800 mesh, which are used in subsequent steps to characterize its structure, morphology, thermodynamic parameters, etc. The amorphous powder particle size distribution data is shown in Table 1. In addition, a -300 mesh powder is screened out for subsequent testing of magnetic properties.
[0061] ① Use an X-ray diffractometer to detect whether the structure of the unscreened original powder and the screened fifth-level powder is amorphous. Figure 2 Fe 73 The X-ray diffraction patterns of the unscreened powder and five grades of powders prepared by aerosolization of P8C7B6Si3Mo3 show diffuse scattering peaks typical of amorphous alloys, without sharp diffraction peaks corresponding to the crystalline structure, indicating that the prepared powder has a completely amorphous structure and can be used for the subsequent preparation of magnetic powder cores and the characterization of soft magnetic properties.
[0062] ② The morphology of the amorphous alloy powder was observed using a scanning electron microscope (SEM). Figure 3 This is a scanning electron microscope photo of amorphous powder with a particle size range of -300-+500 mesh. It can be seen that the powder is spherical and has a smooth surface.
[0063] ③ Differential scanning calorimetry (DSC) was used to measure the Fe 73 Thermal analysis of P8C7B6Si3Mo3 amorphous powder, DSC curve as shown Figure 4 As shown, the glass transition temperature (T g ) and the initial crystallization temperature (T x ), the specific values are shown in Table 1.
[0064] ④ The saturation magnetization intensity (M) of the amorphous powder was measured using a vibrating sample magnetometer (VSM). s ) (maximum external magnetic field is 800kA / m), the results are shown in Table 1. The hysteresis loop is as follows Figure 5 shown.
[0065] Among them, the critical dimensions of the iron-based amorphous soft magnetic alloy rods are shown in Table 2, the performance test results of the iron-based amorphous soft magnetic alloy strips are shown in Table 2, and the performance test results of the iron-based amorphous soft magnetic alloy powders are shown in Table 1.
[0066] Example 2
[0067] This embodiment provides an iron-based amorphous soft magnetic alloy having the general formula Fe 74 P7C7B7Si3Mo1Cr1;
[0068] This embodiment also provides a method for preparing an iron-based amorphous soft magnetic alloy rod having a general formula of Fe 74 P7C7B7Si3Mo1Cr1, the preparation method comprises the following steps:
[0069] Fe, Mo, Cr, Si with a purity greater than 99.5wt.% and FeC, FeB, FeP with a purity greater than 99wt.% are prepared according to a general formula to obtain a raw material mixture. An induction melting furnace is used, the cavity is evacuated and filled with argon gas, and the raw material mixture is repeatedly melted 4 times to ensure uniform composition, and a master alloy ingot is obtained for standby use.
[0070] The master alloy ingot is placed in a quartz crucible with a nozzle, heated to above the melting point, and when the alloy is completely melted, 0.05MPa argon is filled into the quartz crucible, and the melt is sprayed into a copper mold with an inner hole size of at least Ф1mm to obtain an alloy rod.
[0071] The cross section of the alloy rod was examined by X-ray diffractometer, such as Figure 1 As shown, there is no obvious crystallization peak under the distinguishable conditions in the spectrum, indicating that the prepared alloy rod has an amorphous structure and is a rod-shaped bulk amorphous alloy material, that is, the alloy has a rod-shaped critical size (referred to as critical size) for forming an amorphous structure of more than 1 mm. The critical size of the iron-based amorphous soft magnetic alloy rod prepared in this embodiment is shown in Table 2.
[0072] This embodiment also provides a method for preparing an iron-based amorphous soft magnetic alloy strip having a general formula of Fe 74 P7C7B7Si3Mo1Cr1, including the following steps:
[0073] The method for preparing the master alloy ingot is the same as above.
[0074] The master alloy ingot is placed in a quartz crucible with a nozzle, heated to above the melting point, and when the alloy is completely melted, 0.05MPa argon gas is injected into the quartz crucible, and the melt is sprayed onto the surface of a copper roller with a rotation speed of 35m / s, and cooled to obtain an amorphous alloy strip. The soft magnetic properties of the amorphous alloy strip are tested by annealing the amorphous alloy strip at 370℃ and testing it under an external field of 800kA / m. The saturation magnetization intensity M of the amorphous alloy strip is s It is 1.34T, tested under an external field of 800A / m, the magnetic induction intensity B 800 1.31T, coercive force H c It is about 1.0A / m. The specific results are shown in Table 2.
[0075] This embodiment also provides a method for preparing an iron-based amorphous soft magnetic alloy powder having a general formula of Fe 74 P7C7B7Si3Mo1Cr1, including the following steps:
[0076] The method for preparing the master alloy ingot is the same as above.
[0077] The master alloy ingot is placed in a crucible in a gas atomization furnace and heated to above the melting point. After the alloy is completely melted, it is atomized under the action of high-pressure argon gas, and after cooling and solidification, fine spherical powder is formed, i.e., amorphous alloy spherical powder; wherein, those skilled in the art can determine the atomization pressure according to the equipment and the melting conditions of the alloy liquid. The amorphous alloy spherical powder is graded using a standard sieve to obtain five levels of powders, i.e., -50-+200 mesh, -200-+300 mesh, -300-+500 mesh, -500-+800 mesh and -800 mesh, which are used in subsequent steps to characterize its structure, morphology, thermodynamic parameters, etc. The amorphous powder particle size distribution data is shown in Table 1. In addition, a -300 mesh powder is screened out for subsequent testing of magnetic properties.
[0078] ① Use an X-ray diffractometer to detect whether the structure of the unscreened original powder and the screened fifth-level powder is amorphous. Figure 6 Fe 74 The X-ray diffraction patterns of the unscreened powder and five grades of powders prepared by aerosolization of P7C7B7Si3Mo1Cr1 show that all patterns have typical diffuse scattering peaks of amorphous alloys, and there are no sharp diffraction peaks corresponding to the crystalline structure, indicating that the prepared powder has a completely amorphous structure and can be used for the subsequent preparation of magnetic powder cores and the characterization of soft magnetic properties.
[0079] ② The morphology of the amorphous alloy powder was observed using a scanning electron microscope (SEM). Figure 7 This is a scanning electron microscope photo of amorphous powder with a particle size range of -300-+500 mesh. It can be seen that the powder is spherical and has a smooth surface.
[0080] ③ Differential scanning calorimetry (DSC) was used to measure the Fe 74 Thermal analysis of P7C7B7Si3Mo1Cr1 amorphous powder, DSC curve as shown Figure 4 As shown, the glass transition temperature (T g ) and the initial crystallization temperature (T x ), the specific values are shown in Table 1.
[0081] ④ The saturation magnetization intensity (M) of the amorphous powder was measured using a vibrating sample magnetometer (VSM). s )(maximum external magnetic field is 800kA / m), the specific values are shown in Table 1, and the hysteresis loop is shown in Figure 5 shown.
[0082] Among them, the critical dimensions of the iron-based amorphous soft magnetic alloy rods are shown in Table 2, the performance test results of the iron-based amorphous soft magnetic alloy strips are shown in Table 2, and the performance test results of the iron-based amorphous soft magnetic alloy powders are shown in Table 1.
[0083] This embodiment also provides a method for preparing a magnetic powder core, comprising the following steps:
[0084] The -300 mesh iron-based amorphous soft magnetic alloy powder sieved above is added to a 4wt.% phosphoric acid solution and phosphated at 50°C for 30 minutes; the phosphated powder is added to a 0.5wt.% KH-550 alcohol aqueous solution and stirred for 5 minutes in a 50°C water bath for coupling; the coupled amorphous powder is added to a silicone resin acetone solution and subjected to insulation treatment, the mass ratio of silicone resin to iron-based amorphous soft magnetic alloy powder is 2:100, stirred until acetone is completely volatilized, that is, the insulation treatment is completed, and vacuum dried to obtain an insulating amorphous powder. The morphology of the insulating amorphous powder is observed by scanning electron microscopy, and the surface of the powder is covered with a layer of coating resin. The mass fraction of silicone resin in the acetone solution is not limited.
[0085] The coated powder was pressed under a pressure of 1000 MPa into a magnetic powder core with an outer diameter of 20 mm and an inner diameter of 12 mm, and the magnetic powder core was annealed in a protective atmosphere at 430° C. for 60 min.
[0086] The AC BH loop tracer was used to test the loss of the prepared magnetic powder core under the conditions of working magnetic induction of 100mT and working frequency of 100kHz; the impedance analyzer was used to test its loss under the conditions of 10 4 -107 Effective permeability μ at Hz frequency e ; The DC bias characteristics at 100kHz were tested using an inductance-capacitance-resistance (LCR) meter. cv(100kHz,100mT) =730kW / m 3 , corresponding to 10 6 The effective permeability at Hz remains at 22, and the DC bias capability at 100Oe is 89%.
[0087] Example 3
[0088] This embodiment provides an iron-based amorphous soft magnetic alloy having the general formula Fe 75 P7C7B7Si3Mo 0.5 Cr 0.5 ;
[0089] This embodiment also provides a method for preparing an iron-based amorphous soft magnetic alloy rod having a general formula of Fe 75 P7C7B7Si3Mo 0.5 Cr 0.5 , the preparation method comprises the following steps:
[0090] The raw material mixture is prepared by using Fe, Mo, Cr, Si with a purity greater than 99.5wt.% and FeC, FeB, FeP with a purity greater than 99wt.% according to the general formula of iron-based amorphous soft magnetic alloy. The raw material mixture is repeatedly smelted 4 times in an induction melting furnace, after the cavity is evacuated and filled with argon gas, to ensure uniform composition, and a master alloy ingot is obtained for standby use.
[0091] The master alloy ingot is placed in a quartz crucible with a nozzle, heated to above the melting point, and when the alloy is completely melted, 0.05MPa argon gas is filled into the quartz crucible, and the melt is sprayed into a copper mold with an inner hole size of at least 1mm to obtain an alloy rod. The cross section of the alloy rod is detected by an X-ray diffractometer. Figure 1 As shown in the figure, there is no obvious crystallization peak. The critical dimensions of the alloy rods are shown in Table 2.
[0092] This embodiment also provides a method for preparing an iron-based amorphous soft magnetic alloy strip having a general formula of Fe 75 P7C7B7Si3Mo 0.5 Cr 0.5 , the preparation method comprises the following steps:
[0093] The method for preparing the master alloy ingot is the same as above.
[0094] The master alloy ingot was placed in a quartz crucible with a nozzle and heated to above the melting point. When the alloy was completely melted, 0.05 MPa argon gas was injected into the quartz crucible, and the melt was sprayed onto the surface of a copper roller with a rotation speed of 35 m / s. The amorphous alloy strip was obtained by cooling, and the soft magnetic properties of the amorphous alloy strip were tested. The amorphous alloy strip was annealed at 370 ° C and tested under an external field of 800 kA / m. The saturation magnetization intensity M s It is 1.41T, tested under an external field of 800A / m, the magnetic induction intensity B 800 1.38T, coercive force H c About 0.7A / m. See Table 2 for specific results.
[0095] Example 4
[0096] This embodiment provides an iron-based amorphous soft magnetic alloy having the general formula Fe 73 P7C7B7Si3Mo1Cr2;
[0097] This embodiment also provides a method for preparing an iron-based amorphous soft magnetic alloy rod, and the preparation method is the same as that of Embodiment 3.
[0098] This embodiment also provides a method for preparing an iron-based amorphous soft magnetic alloy powder. The preparation method is the same as that of Embodiment 3.
[0099] Example 5
[0100] This embodiment provides an iron-based amorphous soft magnetic alloy having the general formula Fe 73 P7C7B7Si3Mo1V2;
[0101] This embodiment also provides a method for preparing an iron-based amorphous soft magnetic alloy rod, and the preparation method is the same as that of Embodiment 3.
[0102] This embodiment also provides a method for preparing an iron-based amorphous soft magnetic alloy powder. The preparation method is the same as that of Embodiment 3.
[0103] Example 6
[0104] This embodiment provides an iron-based amorphous soft magnetic alloy having the general formula Fe 74 P7C7B7Si3Mo1V1;
[0105] This embodiment also provides a method for preparing an iron-based amorphous soft magnetic alloy rod, and the preparation method is the same as that of Embodiment 3.
[0106] This embodiment also provides a method for preparing an iron-based amorphous soft magnetic alloy powder. The preparation method is the same as that of Embodiment 3.
[0107] Example 7
[0108] This embodiment provides an iron-based amorphous soft magnetic alloy having the general formula Fe 71 P7C7B7Si3Mo5;
[0109] This embodiment also provides a method for preparing an iron-based amorphous soft magnetic alloy rod, and the preparation method is the same as that of Embodiment 3.
[0110] This embodiment also provides a method for preparing an iron-based amorphous soft magnetic alloy powder. The preparation method is the same as that of Embodiment 3.
[0111] Example 8
[0112] This embodiment provides an iron-based amorphous soft magnetic alloy having the general formula Fe 72 P7C7B7Si3Mo4;
[0113] This embodiment also provides a method for preparing an iron-based amorphous soft magnetic alloy rod, and the preparation method is the same as that of Embodiment 3.
[0114] This embodiment also provides a method for preparing an iron-based amorphous soft magnetic alloy powder. The preparation method is the same as that of Embodiment 3.
[0115] Example 9
[0116] This embodiment provides an iron-based amorphous soft magnetic alloy having the general formula Fe 73 P7C7B7Si3Mo3;
[0117] This embodiment also provides a method for preparing an iron-based amorphous soft magnetic alloy rod, and the preparation method is the same as that of Embodiment 3.
[0118] This embodiment also provides a method for preparing an iron-based amorphous soft magnetic alloy powder. The preparation method is the same as that of Embodiment 3.
[0119] Example 10
[0120] This embodiment provides an iron-based amorphous soft magnetic alloy having the general formula Fe 74 P7C7B7Si3Mo2;
[0121] This embodiment also provides a method for preparing an iron-based amorphous soft magnetic alloy rod, and the preparation method is the same as that of Embodiment 3.
[0122] This embodiment also provides a method for preparing an iron-based amorphous soft magnetic alloy powder. The preparation method is the same as that of Embodiment 3.
[0123] Embodiment 11
[0124] This embodiment provides an iron-based amorphous soft magnetic alloy having the general formula Fe 75 P7C7B7Si3Mo1;
[0125] This embodiment also provides a method for preparing an iron-based amorphous soft magnetic alloy rod, and the preparation method is the same as that of Embodiment 3.
[0126] This embodiment also provides a method for preparing an iron-based amorphous soft magnetic alloy powder. The preparation method is the same as that of Embodiment 3.
[0127] Example 12
[0128] This embodiment provides an iron-based amorphous soft magnetic alloy having the general formula Fe 75.5 P7C7B7Si3Mo 0.5 ;
[0129] This embodiment also provides a method for preparing an iron-based amorphous soft magnetic alloy rod, and the preparation method is the same as that of Embodiment 3.
[0130] This embodiment also provides a method for preparing an iron-based amorphous soft magnetic alloy powder. The preparation method is the same as that of Embodiment 3.
[0131] Embodiment 13
[0132] This embodiment provides an iron-based amorphous soft magnetic alloy having the general formula Fe 76 P7C7B7Si3;
[0133] This embodiment also provides a method for preparing an iron-based amorphous soft magnetic alloy rod, and the preparation method is the same as that of Embodiment 3.
[0134] This embodiment also provides a method for preparing an iron-based amorphous soft magnetic alloy powder. The preparation method is the same as that of Embodiment 3.
[0135] Embodiment 14
[0136] This embodiment provides an iron-based amorphous soft magnetic alloy having the general formula Fe 76 P3C4B 11 Si3Mo3;
[0137] This embodiment also provides a method for preparing an iron-based amorphous soft magnetic alloy rod, and the preparation method is the same as that of Embodiment 3.
[0138] This embodiment also provides a method for preparing an iron-based amorphous soft magnetic alloy powder. The preparation method is the same as that of Embodiment 3.
[0139] Embodiment 15
[0140] This embodiment provides an iron-based amorphous soft magnetic alloy having the general formula Fe 73 P4C9B8Si3Mo3;
[0141] This embodiment also provides a method for preparing an iron-based amorphous soft magnetic alloy rod, and the preparation method is the same as that of Embodiment 3.
[0142] This embodiment also provides a method for preparing an iron-based amorphous soft magnetic alloy powder. The preparation method is the same as that of Embodiment 3.
[0143] Example 16
[0144] This embodiment provides an iron-based amorphous soft magnetic alloy having the general formula Fe 73 P4C 12 B5Si3Mo3;
[0145] This embodiment also provides a method for preparing an iron-based amorphous soft magnetic alloy rod, and the preparation method is the same as that of Embodiment 3.
[0146] This embodiment also provides a method for preparing an iron-based amorphous soft magnetic alloy powder. The preparation method is the same as that of Embodiment 3.
[0147] Embodiment 17
[0148] This embodiment provides an iron-based amorphous soft magnetic alloy having the general formula Fe 73 P5C 10 B6Si3Mo3;
[0149] This embodiment also provides a method for preparing an iron-based amorphous soft magnetic alloy rod, and the preparation method is the same as that of Embodiment 3.
[0150] This embodiment also provides a method for preparing an iron-based amorphous soft magnetic alloy powder. The preparation method is the same as that of Embodiment 3.
[0151] Embodiment 18
[0152] This embodiment provides an iron-based amorphous soft magnetic alloy having the general formula Fe 73 P6C5B 10 Si3Mo3;
[0153] This embodiment also provides a method for preparing an iron-based amorphous soft magnetic alloy rod, and the preparation method is the same as that of Embodiment 3.
[0154] This embodiment also provides a method for preparing an iron-based amorphous soft magnetic alloy powder. The preparation method is the same as that of Embodiment 3.
[0155] Embodiment 19
[0156] This embodiment provides an iron-based amorphous soft magnetic alloy having the general formula Fe 73 P6C9B6Si3Mo3;
[0157] This embodiment also provides a method for preparing an iron-based amorphous soft magnetic alloy rod, and the preparation method is the same as that of Embodiment 3.
[0158] This embodiment also provides a method for preparing an iron-based amorphous soft magnetic alloy powder. The preparation method is the same as that of Embodiment 3.
[0159] Embodiment 20
[0160] This embodiment provides an iron-based amorphous soft magnetic alloy having the general formula Fe 73 P6C8B7Si3Mo3;
[0161] This embodiment also provides a method for preparing an iron-based amorphous soft magnetic alloy rod, and the preparation method is the same as that of Embodiment 3.
[0162] This embodiment also provides a method for preparing an iron-based amorphous soft magnetic alloy powder. The preparation method is the same as that of Embodiment 3.
[0163] Comparative Example 1
[0164] This comparative example provides an iron-based amorphous soft magnetic alloy powder having the general formula Fe 73.5 B9 13.5 Cu1Nb3; The preparation method of the iron-based amorphous soft magnetic alloy powder is the same as that of Example 1. Figure 8 The X-ray diffraction patterns of three levels of powders sieved through -300-+500 mesh, -500-+800 mesh, and -800-+900 mesh in this comparative example. Sharp diffraction peaks appeared in the spectrum, indicating that the component is Fe 73.5 B9 13.5 The alloy-forming ability of Cu1Nb3 is low, and it is impossible to prepare a completely amorphous powder.
[0165] Table 1 Performance test results of amorphous alloy powders prepared in Example 1 and Example 2
[0166]
[0167] Table 2 Performance test results of amorphous alloy rods and amorphous alloy strips prepared in Examples 1-20
[0168]
[0169]
[0170] Among them, D in Table 2 c is the critical size of the amorphous alloy rod; T g , T x 、M s , H c , B 800 These are the performance test results of amorphous alloy strips.
[0171] It can be seen from Table 1-2 that the iron-based amorphous soft magnetic alloy provided by the present invention has a low coercive force H c , the minimum can be 0.6±0.2A / m, saturation magnetization intensity M sThe maximum is 1.5T, B 800 ≥1.0T.
[0172] The critical size can be further increased by adding Mo, Cr or V to the Fe-based amorphous soft magnetic alloy.
[0173] Obviously, the above embodiments are merely examples for the purpose of clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived from these are still within the scope of protection of the invention.
Claims
1. An iron-based amorphous soft magnetic alloy, characterized in that: It has the general formula shown in Formula I, Fe (100-a-b-c-d-e-f) P a C b B c Si d Mo e N f , formula I wherein a, b, c, d, e, and f respectively represent the atomic percentages of P, C, B, Si, Mo, and N. Based on 100% of the atomic percentage, a% + b% + c% + d% + e% + f% = 100%; the value ranges of a, b, c, d, e, and f are 3 ≤ a ≤ 8, 4 ≤ b ≤ 12, 5 ≤ c ≤ 11, 2.8 ≤ d ≤ 3.2, 0 ≤ e ≤ 5, and 0 ≤ e + f ≤ 5; N is at least one of Cr and V.
2. The iron-based amorphous soft magnetic alloy according to claim 1, characterized in that: When 4 ≤ b ≤ 6, f < 1; When 6 < b ≤ 12, 0 ≤ f ≤ 2.
3. The iron-based amorphous soft magnetic alloy according to claim 1 or 2, characterized in that: The iron-based amorphous soft magnetic alloy is an alloy bulk, alloy strip, or alloy powder.
4. A method for preparing an iron-based amorphous soft magnetic alloy powder, characterized in that: The composition of the iron-based amorphous soft magnetic alloy powder is selected from the iron-based amorphous soft magnetic alloy described in Claim 1 or 2, and the preparation method includes the following steps: Ingredient preparation; Melting to obtain a master alloy ingot; Melting the master alloy ingot, atomizing it by the gas atomization method, and obtaining the iron-based amorphous soft magnetic alloy powder after solidification.
5. A method for preparing a magnetic powder core, characterized in that: The iron-based amorphous soft magnetic alloy powder prepared by the preparation method described in Claim 4 includes the following steps: Successively performing phosphating, coupling, and insulation treatments on the iron-based amorphous soft magnetic alloy powder, and then performing cold pressing and heat treatment on it.
6. The preparation method according to claim 5, characterized in that: Performing phosphating treatment on the powder with a phosphating solution; Preferably, the treatment time of the phosphating is 30 - 60 min, and the temperature is 40 - 60 °C; Preferably, the phosphating solution is a phosphoric acid solution.
7. The preparation method according to claim 5 or 6, characterized in that: Performing the coupling with a silane coupling agent; preferably, the coupling time is 5 - 10 min, and the temperature is 40 - 60 °C; Preferably, performing the insulation treatment with an organosilicon resin, epoxy resin, or polytetrafluoroethylene.
8. The preparation method according to any one of claims 5 to 7, characterized in that: The pressure of the cold pressing is 500 - 2000 MPa, and the time is 5 - 10 min; Preferably, the specific steps of the heat treatment include holding for at least 1 h in a protective atmosphere at 300 - 500 °C; Preferably, the protective atmosphere is at least one of argon and nitrogen.
9. The magnetic powder core obtained by the preparation method according to any one of claims 5 to 8.