Magnetron sputtering coating device and coating method for continuous fiber surface
By designing a magnetron sputtering coating device for the surface of continuous fibers and using the spiral winding technology of arc-shaped circular plates and godets, the shadow effect and continuity problems of fiber surface coatings in magnetron sputtering technology have been solved, achieving Full coverage and efficient coating improve fiber performance.
Patent Information
- Application Number
- CN202310304927.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-27
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2043-03-27
AI Technical Summary
Existing magnetron sputtering technology has problems such as shadow effects and inability to ensure coating continuity when coating the surface of continuous fibers, resulting in uneven film coverage and limited performance.
A magnetron sputtering coating device for the surface of continuous fibers is designed, including a three-dimensional winding system, a power and transmission system and a control system. The spiral three-dimensional winding of the fiber is realized through an arc-shaped circular plate and a godet wheel. Combined with the positive movement of the motor, , inversion controls the reciprocating motion of the fiber to ensure full surface coverage and continuous coating.
It achieves full coverage and continuity of fiber surface coating. By regulating parameters such as motor speed, sputtering power and temperature, it effectively controls the structure and performance of the film, reduces costs and simplifies the device structure.
Smart Images

Figure CN116288212B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of material manufacturing and relates to a magnetron sputtering coating device for a continuous fiber surface.
[0002] The invention also relates to a magnetron sputtering coating method for the surface of continuous fibers. Background Art
[0003] Fiber surface coating technology is to deposit metal or compound films on the fiber surface through related processes, which can effectively improve the various properties of the fiber in practical applications. Among the fiber coating methods, chemical vapor deposition requires a certain reaction temperature and the composition and structure of the reaction products are difficult to control. The density and uniformity of the film are poor, and it is easy to contaminate the fiber, which limits the thin film system prepared by this method. Physical vapor deposition methods include thermal evaporation, arc ion plating and magnetron sputtering, which can prepare thin films under lower temperature conditions. Among them, magnetron sputtering is an advanced coating technology. The thin film prepared by this method has uniform structure, fine grains, good bonding with fibers and excellent performance.
[0004] By using magnetron sputtering technology to coat the fiber surface, almost all metals, alloys and compound materials can be deposited on the fiber surface according to different needs. Under appropriate conditions, multi-target co-sputtering can also be used to control the composition and structure of the film. Adding nitrogen or other active gases to the sputtering atmosphere can deposit and form the corresponding compound film. In addition, by controlling the sputtering time, power, temperature, working gas pressure and atmosphere flow, the thickness, structure morphology and performance of the fiber surface film can be controlled.
[0005] There are relatively few reports on the field of continuous fiber surface coating using existing magnetron sputtering technology. The main reason is that magnetron sputtering equipment has an insurmountable shadow effect during coating, which makes it impossible to coat the fiber surface below. At the same time, due to the limitation of fiber length, the continuity of fiber surface coating cannot be guaranteed. Therefore, it is of great practical value to develop a continuous fiber surface coating device and method for magnetron sputtering. Summary of the invention
[0006] The purpose of the present invention is to provide a magnetron sputtering coating device for continuous fiber surfaces, which solves the problem in the prior art that the continuity of the fiber surface coating cannot be guaranteed due to the limitation of the fiber length.
[0007] Another object of the present invention is to provide a method for magnetron sputtering coating on the surface of continuous fibers.
[0008] The technical solution adopted by the present invention is that the magnetron sputtering coating device for the surface of continuous fibers comprises a base support and an upper support arranged on the base support, and the upper support is respectively provided with a three-dimensional winding system, a power and transmission system and a control system;
[0009] The three-dimensional winding system includes a wire feeding reel and a wire collecting reel symmetrically arranged at both ends of the upper support, the wire feeding reel and the wire collecting reel are respectively connected to the power system, the upper support is located at the symmetric center of the wire feeding reel and the wire collecting reel and is provided with an arc-shaped circular plate, a plurality of wire guide wheels are arranged in the arc-shaped circular plate, and the fiber passes through the wire feeding reel, the wire guide wheel and the wire collecting reel in sequence;
[0010] The power system includes a motor for driving a wire feeding reel and a wire taking-up reel;
[0011] The control system is a signal receiving and control unit, and the signal receiving and control unit is connected to the motor of the power system.
[0012] The first technical solution of the present invention is also characterized in that:
[0013] The arc-shaped circular plate is provided with gaps at both ends close to the wire feeding reel and the wire collecting reel, and the gaps are movably connected to the winding roller and the wire collecting reel respectively;
[0014] Wherein a plurality of the guide wire wheels are evenly distributed around the arc surface of the arc-shaped circular plate.
[0015] The wire guide wheel includes a rotating wheel, which is movably connected to a U-shaped wheel frame. The two ends of the wheel frame opening are movably connected to the two sides of the rotating wheel. A circular disc with a hole is provided at the closed end of the wheel frame. A mounting rod is embedded in the hole of the circular disc with a hole. The mounting rod points to the rotating wheel, and a spring is sleeved on the rod body of the mounting rod pointing to the rotating wheel. The rotating wheel is a small radius V-groove wheel.
[0016] The power system includes a motor and a motor A connected to the wire feeding drum and the wire collecting drum respectively, the motor and the motor A are fixed between the base bracket and the upper support respectively, the motor is connected to the wire feeding drum through a coupling, a wire feeding shaft worm gear, and a worm transmission shaft in sequence, the motor A is connected to the wire collecting drum through a coupling A, a wire collecting shaft worm gear A, and a worm transmission shaft A in sequence, the end of the worm transmission shaft away from the wire feeding shaft worm gear is connected to the bearing support, and the end of the worm transmission shaft A away from the wire collecting shaft worm gear A is connected to the bearing support A;
[0017] The control system further includes a limit sensing unit and a limit sensing unit A respectively arranged on the upper support, the limit sensing unit and the limit sensing unit A are respectively connected to the signal receiving and control unit, and the limit sensing unit and the limit sensing unit A are respectively located at the wire outlet of the wire feeding reel and the wire receiving reel;
[0018] A fiber tensioning mechanism and a fiber tensioning mechanism A are respectively provided between the wire feeding reel and the wire taking-up reel and the winding roller and the wire taking-up reel;
[0019] The barrels of the wire feeding reel and the wire collecting reel are respectively provided with a fiber clamping mechanism and a fiber clamping mechanism A.
[0020] The second technical solution adopted by the present invention is a method for magnetron sputtering coating on the surface of a continuous fiber, which adopts a magnetron sputtering coating device on the surface of a continuous fiber and is specifically implemented in the following steps:
[0021] Step 1, soak the fiber in anhydrous ethanol, clean it in an ultrasonic cleaner for 10 minutes and then set it aside;
[0022] Step 2, winding one end of the fiber on the wire feeding drum, then winding the fiber around the fiber tensioning mechanism and the wire feeding roller, and then winding the fiber around several groups of wire guide wheels in a spatial spiral winding manner, and then winding the fiber from the wire taking-up roller and winding it on the wire taking-up drum. After the pre-winding is completed, the wire taking-up drum is rotated so that the fiber is in a tensioned state;
[0023] Step 3: Fix the winding system on the loading plate of the magnetron sputtering device through C-type clamps and C-type clamps A, close the magnetron sputtering chamber, and first perform low vacuum extraction. When the pressure in the sputtering chamber reaches below 4 Pa, perform high vacuum extraction. When the vacuum degree in the sputtering chamber reaches the predetermined value of 7×10 -4 After Pa, argon gas is introduced at 50 sccm and pre-sputtering is performed for 10 minutes. After power-on sputtering, the motor and motor A are started to drive the fiber to be wound along the preset route and surface coating begins. When the fiber on the reel is fed to the specified position, the motor is controlled to reverse and drive the fiber to be wound. After the fiber is reciprocated and coated on the three-dimensional winding device for 10 times, the motor and motor A are turned off, the sputtering is stopped, and the sample is taken out after it has cooled to room temperature with the furnace.
[0024] The second technical solution of the present invention is also characterized in that:
[0025] The rotation speeds of the motor and the motor A are 5 to 100 rpm, the reduction ratios of the worm gears connected thereto are 1:15, the sputtering power in the magnetron sputtering is 50 to 300 W, and the substrate temperature is 20 to 500° C.
[0026] The beneficial effects of the present invention are:
[0027] The continuous fiber surface magnetron sputtering coating device of the present invention has low cost, simple and reliable structure, can be conveniently installed in the cavity of the magnetron sputtering equipment, and has positive practical value for the surface modification and performance improvement of the fiber;
[0028] The method for magnetron sputtering coating on the surface of continuous fibers of the present invention performs magnetron sputtering coating on the fibers, wherein the fibers are spirally wound three-dimensionally, and the reciprocating motion of the fibers is controlled by the forward and reverse rotation of the motor, thereby ensuring both full surface coverage of the fiber coating and the continuity of the fiber surface coating. During the sputtering process, the organizational structure, thickness and performance of the film can be effectively regulated by controlling process parameters such as the motor speed, the number of forward and reverse rotations of the motor, the sputtering power, the substrate temperature and the sputtering time. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 It is a three-dimensional structural diagram of the magnetron sputtering coating device on the surface of the continuous fiber of the present invention;
[0030] Figure 2 It is a side view of the magnetron sputtering coating device for the surface of the continuous fiber of the present invention;
[0031] Figure 3 It is a three-dimensional wire winding schematic diagram of the magnetron sputtering coating device on the surface of the continuous fiber of the present invention;
[0032] Figure 4 It is a structural diagram of the guide wire wheel of the magnetron sputtering coating device for the surface of continuous fibers of the present invention;
[0033] Figure 5 This is a physical picture of the magnetron sputtering coating device for the continuous fiber surface of the present invention.
[0034] In the figure, 1. base bracket, 2. upper support, 3. wire feeding drum, 4. wire feeding drum shaft, 5. fiber clamping mechanism, 15. fiber clamping mechanism A, 6. limit sensing unit, 14. limit sensing unit A, 7. fiber tensioning mechanism, 13. fiber tensioning mechanism A, 8. wire feeding roller, 9. arc circular plate, 10. wire guide wheel, 11. fiber, 12. wire collection roller, 16. wire collection drum shaft, 17. wire collection drum, 18. motor, 19. coupling, 28. Coupling A, 20. Wire feeding shaft worm gear, 21. Worm transmission shaft, 26. Worm transmission shaft A, 22. Bearing support, 25. Bearing support A, 23. Magnetron sputtering target sputtering source, 24. Magnetron sputtering carrier disc, 27. Wire receiving shaft worm gear, 29. Motor A, 30. Signal receiving and control unit, 31. C-type fixing clamp, 32. C-type fixing clamp A, 33. Rotating wheel, 34. Wheel frame, 35. Splash plate, 36. Spring, 37. Mounting rod. DETAILED DESCRIPTION
[0035] The present invention is described in detail below with reference to the accompanying drawings and specific embodiments.
[0036] The present invention provides a continuous fiber surface magnetron sputtering coating device, comprising a fiber, a target material sputtering source 23, a magnetron sputtering carrier disc 24 and a continuous fiber surface coating device; the carrier disc is fixed with a fiber surface coating device, including a three-dimensional winding system, a power and transmission system and a control system, etc.; during the sputtering process, ionized argon ions and electrons bombard the target material so that the target material surface material is bombarded out, and finally a thin film is formed on the fiber surface in the arc-shaped circular plate area of the device;
[0037] like Figure 1 and Figure 2As shown, the winding system consists of a wire feeding drum 3, a wire feeding roller 8, an arc-shaped circular plate 9, a wire guide wheel 10, a wire collection roller 12, and a wire collection drum 17; wherein the wire feeding drum 3 and the wire collection drum 17 are symmetrically mounted on the upper support 2 and connected to the power system, the roller 8 and the wire collection roller 12 are fixed on the upper support 2 and rotated to guide the fiber, and the arc-shaped circular plate 9 serves to fix a plurality of wire guide wheels 10; as shown Figure 4 As shown, the wire guide wheel 10 is a combination, which consists of a rotating wheel 33, a wheel frame 34, a splash plate 35, a spring 36 and a mounting rod 37, wherein the rotating wheel 33 is mounted on the wheel frame 34 for rotation, and a splash plate 35 fixed to the bracket is placed above the rotating wheel 33; at the same time, one end of the mounting rod 37 equipped with a spring 36 passes through the perforated disc on the wheel frame 34, which can adjust the tension of the fiber 11 running on the device to ensure that the fiber is in a tensioned state during the movement; Figure 3 As shown, the runner 33 is a small radius V-groove wheel, and the height difference between the fiber entering the runner and the fiber leaving the runner is small, ensuring that the distance between different parts of the fiber in the sputtering area and the sputtering source is not much different; the fiber is spirally three-dimensionally wound by the guide wire wheel, overcoming the shadow effect in the magnetron sputtering process, and ensuring uniform deposition of thin film on the fiber surface;
[0038] The power and transmission system is composed of a motor 18, a motor A29, a wire feeding shaft worm wheel 20, a wire collecting shaft worm wheel 27, a worm transmission shaft 21, and a worm transmission shaft A26. The motor 18 and the motor A29 are fixed on the side ribs between the base bracket 1 and the upper support 2, and the worm is driven to rotate through the coupling 19 and the coupling A28; the wire feeding shaft worm wheel 20 and the wire collecting shaft worm wheel 27 have the same number of teeth and module parameters, and are meshed with the worm;
[0039] The signal receiving and control unit 30 of the control system is installed on the upper support 2. After the magnetron sputtering equipment is vacuumed and the atmosphere is ventilated, the signal receiving unit receives external signals to control the motor to drive the fiber movement. The upper support 2 is provided with a fiber limit sensing unit 6 and a fiber limit sensing unit A14. When the fiber completes a cycle of coating, the two motors are controlled to reverse at the same time to carry out the next cycle of coating.
[0040] To ensure that the fiber can move stably, a fiber tensioning mechanism 7 and a fiber tensioning mechanism A13 are provided on both sides of the winding system; a fiber clamping mechanism 5 and a fiber clamping mechanism A15 are provided on the wire feeding reel 3 and the wire receiving reel 17 to prevent the fiber from falling off the reel during winding;
[0041] like Figure 5As shown, during the sputtering process, the fiber is wound onto the device, and then the device is installed on the magnetron sputtering carrier plate 24. The full surface coating of the fiber is achieved through the three-dimensional spiral winding movement of the fiber in the arc-shaped circular plate 9. The motor is controlled to rotate forward and reverse, and the fiber performs reciprocating motion to achieve continuous coating of the fiber. The motor speed is 5 to 100 rpm, the reduction ratio of the worm gear is 1:15, and the conditions for magnetron sputtering are: the sputtering gas is argon, the sputtering power is 50 to 300 W, and the substrate temperature is 20 to 500 ° C.
[0042] The present invention also provides a magnetron sputtering coating method for the surface of a continuous fiber, which is specifically implemented according to the following steps:
[0043] Step 1, soak the fiber in anhydrous ethanol, clean it in an ultrasonic cleaner for 10 minutes and then set it aside;
[0044] Step 2, then remove the wire reel 3 of the device from the shaft, wind the ultrasonically cleaned fiber on the wire feeding reel 3 and insert it into the wire feeding reel shaft 4, then pass the fiber around the fiber tensioning mechanism 7 and then the wire feeding reel 8, then pass the fiber around several groups of wire guide wheels 10 in a spiral manner, then send it out from the wire taking-up reel 12 and wind it on the wire taking-up reel 17, after the pre-winding is completed, rotate the wire taking-up reel 17 to tighten the spring 36, so that the fiber is in a tensioned state;
[0045] Step 3, fix the prepared device on the loading plate 24 of the magnetron sputtering equipment using C-clamps 31 and C-clamps A32, close the magnetron sputtering vacuum chamber, and evacuate. After reaching the preset vacuum degree, set the process parameters such as atmosphere flow rate, working air pressure, sputtering power, substrate temperature and sputtering time; when starting sputtering, set the motor speed and start the motor, drive the worm to rotate through the coupling, and the worm drives the worm wheel and the reel to rotate synchronously, and the fibers in the arc-shaped circular plate 9 move in a spiral manner, and the surface begins to be coated; when the fibers on the wire feeding reel 3 are fed to the limited position, control the motor to rotate in the opposite direction, and drive the wire collection reel 17 to reverse through the transmission system to continue coating; in this way, the fibers are reciprocated during the spiral three-dimensional winding process, thereby ensuring the continuity and uniformity of the fiber coating.
[0046] Example 1
[0047] The fiber is soaked in anhydrous ethanol, cleaned by an ultrasonic cleaner for 10 minutes and then used for later use; one end of the fiber is wound on the wire feeding drum 3, and then the fiber is wound around the fiber tensioning mechanism 7 and the wire feeding roller 8, and then the fiber 11 is wound around several groups of guide wheels 10 in sequence in a spatial spiral winding manner, and then drawn out from the wire taking-up roller 12 and wound on the wire taking-up drum 17. After the pre-winding is completed, the wire taking-up drum 17 is rotated to make the fiber in a tensioned state;
[0048] The winding system is fixed on the carrier plate 24 of the magnetron sputtering device through C-type clamps 31 and A32. The magnetron sputtering chamber is closed. Low vacuum extraction is first performed. When the pressure in the sputtering chamber reaches below 4 Pa, high vacuum extraction is performed. When the vacuum degree in the sputtering chamber reaches the predetermined value of 7×10 -4 After Pa, introduce argon gas at 50sccm and pre-sputter for 10min to remove contaminants on the target surface; set the substrate temperature to 100℃ and the sputtering power to 50W. After power-on sputtering, start motor 18 and motor A29 at a speed of 20 rpm to drive the fiber to wind along a preset route and start surface coating; when the fiber on the wire feeding reel 3 is fed to a limited position, control the motor to reverse and drive the fiber to wind; when the fiber is reciprocated and coated on the three-dimensional winding device for 10 times, turn off motor 18 and motor A29, stop sputtering, and take out the sample after the sample is cooled to room temperature with the furnace.
[0049] Example 2
[0050] The fiber is soaked in anhydrous ethanol, cleaned by an ultrasonic cleaner for 10 minutes and then used for later use; one end of the fiber is wound on the wire feeding drum 3, and then the fiber is wound around the fiber tensioning mechanism 7 and the wire feeding roller 8, and then the fiber 11 is wound around several groups of guide wheels 10 in sequence in a spatial spiral winding manner, and then drawn out from the wire taking-up roller 12 and wound on the wire taking-up drum 17. After the pre-winding is completed, the wire taking-up drum 17 is rotated to make the fiber in a tensioned state;
[0051] The winding system is fixed on the carrier plate 24 of the magnetron sputtering device through C-type clamps 31 and A32, and the magnetron sputtering chamber is closed. Low vacuum extraction is first performed. When the pressure in the sputtering chamber reaches below 4 Pa, high vacuum extraction is performed. When the vacuum degree in the sputtering chamber reaches the predetermined value of 7×10 -4 After Pa, introduce 50sccm of argon and pre-sputter for 10min to remove contaminants on the target surface; set the substrate temperature to 200℃ and the sputtering power to 50W. After power-on sputtering, start motor 18 and motor A29 at a speed of 10 rpm to drive the fiber to wind along a preset route and start surface coating; when the fiber on the wire feeding reel 3 is fed to a limited position, control the motor to reverse and drive the fiber to wind; when the fiber is reciprocated and coated on the three-dimensional winding device for 10 times, turn off motor 18 and motor A29, stop sputtering, and take out the sample after it cools to room temperature with the furnace.
[0052] Example 3
[0053] The fiber is soaked in anhydrous ethanol, cleaned by an ultrasonic cleaner for 10 minutes and then used for later use; one end of the fiber is wound on the wire feeding drum 3, and then the fiber is wound around the fiber tensioning mechanism 7 and the wire feeding roller 8, and then the fiber 11 is wound around several groups of guide wheels 10 in sequence in a spatial spiral winding manner, and then drawn out from the wire taking-up roller 12 and wound on the wire taking-up drum 17. After the pre-winding is completed, the wire taking-up drum 17 is rotated to make the fiber in a tensioned state;
[0054] The winding system is fixed on the carrier plate 24 of the magnetron sputtering device through C-type clamps 31 and A32. The magnetron sputtering chamber is closed. Low vacuum extraction is first performed. When the pressure in the sputtering chamber reaches below 4 Pa, high vacuum extraction is performed. When the vacuum degree in the sputtering chamber reaches the predetermined value of 7×10 -4 After Pa, introduce 50sccm of argon and pre-sputter for 10min to remove contaminants on the target surface; set the substrate temperature to 100℃ and the sputtering power to 50W. After power-on sputtering, start motor 18 and motor A29 at a speed of 50 rpm to drive the fiber to wind along a preset route and start surface coating; when the fiber on the wire-collecting reel 3 is fed to a limited position, control the motor to reverse and drive the fiber to wind; after the fiber is reciprocated and coated on the three-dimensional winding device for 20 times, turn off motor 18 and motor A29, stop sputtering, and take out the sample after it has cooled to room temperature with the furnace.
Claims
1. A magnetron sputtering coating device for continuous fiber surface, characterized in that: It comprises a base support (1) and an upper support (2) arranged on the base support (1), wherein the upper support (2) is respectively provided with a three-dimensional winding system, a power and transmission system, and a control system; The three-dimensional winding system comprises a wire feeding reel (3) and a wire collecting reel (17) symmetrically arranged at two ends of an upper support (2); the wire feeding reel (3) and the wire collecting reel (17) are respectively connected to a power system; an arc-shaped circular plate (9) is arranged at the symmetrical center of the wire feeding reel (3) and the wire collecting reel (17); a plurality of wire guide wheels (10) are arranged in the arc-shaped circular plate (9); and the fiber passes through the wire feeding reel (3), the wire guide wheel (10) and the wire collecting reel (17) in sequence; The power system comprises a motor for driving a wire feeding reel (3) and a wire receiving reel (17); The control system is a signal receiving and control unit (30), and the signal receiving and control unit (30) is connected to the motor of the power system; The wire guide wheel (10) comprises a rotating wheel (33), the rotating wheel (33) is movably connected to a U-shaped wheel frame (34), the two open ends of the wheel frame (34) are movably connected to the two sides of the rotating wheel (33), the closed end of the wheel frame (34) is provided with a perforated disc, the hole of the perforated disc is embedded with a mounting rod (37), the mounting rod (37) points to the rotating wheel (33), and a spring (36) is sleeved on the rod body of the mounting rod (37) pointing to the rotating wheel (33), the rotating wheel (33) is a small radius V-groove wheel, and the wheel frame (34) is located above the rotating wheel (33) and is also provided with a splash plate (35).
2. The magnetron sputtering coating device for continuous fiber surface according to claim 1, characterized in that: The arc-shaped circular plate (9) is provided with notches at both ends close to the wire feeding reel (3) and the wire collecting reel (17), and the reel (8) and the wire collecting reel (12) are movably connected at the notches.
3. The magnetron sputtering coating device for continuous fiber surface according to claim 1, characterized in that: The plurality of guide wire wheels (10) are evenly distributed around the arc surface of the arc-shaped circular plate (9).
4. The magnetron sputtering coating device for continuous fiber surface according to claim 1, characterized in that: The power system comprises a motor (18) and a motor A (29) respectively connected to the wire feeding reel (3) and the wire collecting reel (17); the motor (18) and the motor A (29) are respectively fixed between the base bracket (1) and the upper support (2); the motor (18) is connected to the wire feeding reel (3) via a coupling (19), a wire feeding shaft worm gear (20), and a worm transmission shaft (21) in sequence; the motor A (29) is connected to the wire collecting reel (17) via a coupling A (28), a wire collecting shaft worm gear A (27), and a worm transmission shaft A (26) in sequence; one end of the worm transmission shaft (21) away from the wire feeding shaft worm gear (20) is connected to a bearing support (22); and one end of the worm transmission shaft (26) away from the wire collecting shaft worm gear A (27) is connected to a bearing support A (25).
5. The magnetron sputtering coating device for continuous fiber surface according to claim 1, characterized in that: The control system further comprises a limit sensing unit (6) and a limit sensing unit A (14) respectively arranged on the upper support (2); the limit sensing unit (6) and the limit sensing unit A (14) are respectively connected to the signal receiving and control unit (30); the limit sensing unit (6) and the limit sensing unit A (14) are respectively located at the wire outlet of the wire feeding reel (3) and the wire receiving reel (17).
6. The magnetron sputtering coating device for continuous fiber surface according to claim 1, characterized in that: A fiber tensioning mechanism (7) and a fiber tensioning mechanism A (13) are provided between the wire feeding reel (3) and the wire collecting reel (17) and the winding roller (8) and the wire collecting reel (12) respectively.
7. The magnetron sputtering coating device for continuous fiber surface according to claim 1, characterized in that: The barrels of the wire feeding reel (3) and the wire collecting reel (17) are respectively provided with a fiber clamping mechanism (5) and a fiber clamping mechanism A (15).
8. A method for magnetron sputtering coating on the surface of a continuous fiber, using the magnetron sputtering coating device for the surface of a continuous fiber according to any one of claims 1 to 7, characterized in that: Please follow the steps below to implement: Step 1, soak the fiber in anhydrous ethanol, clean it in an ultrasonic cleaner for 10 minutes and then set it aside; Step 2, winding one end of the fiber on the wire feeding drum (3), then winding the fiber filament around the fiber tensioning mechanism (7) and the wire feeding roller (8), then winding the fiber (11) around a plurality of groups of guide wheels (10) in a spatial spiral winding manner, and then leading the fiber from the wire taking-up roller (12) and winding it on the wire taking-up drum (17), and rotating the wire taking-up drum (17) after the pre-winding is completed, so that the fiber is in a tensioned state; Step 3, fix the winding system on the loading plate (24) of the magnetron sputtering device through the C-type clamp (31) and the C-type clamp A (32), close the magnetron sputtering chamber, first perform low vacuum extraction, and when the pressure in the sputtering chamber reaches below 4 Pa, perform high vacuum extraction; when the vacuum degree in the sputtering chamber reaches a predetermined value of 7×10 -4 After Pa, argon gas is introduced at 50 sccm and pre-sputtering is performed for 10 minutes; after power is turned on for sputtering, the motor (18) and the motor A (29) are started to drive the fiber to be wound along a preset route and start surface coating. When the fiber on the wire feeding reel (3) is fed to a specified position, the motor (18) is controlled to reverse and drive the fiber to be wound. After the fiber is reciprocated and coated on the three-dimensional winding device for 10 times, the motor (18) and the motor A (29) are turned off, the sputtering is stopped, and the sample is taken out after it is cooled to room temperature with the furnace.
9. The method for magnetron sputtering coating on the surface of continuous fibers according to claim 8, characterized in that: The rotation speed of the motor (18) and the motor A (29) is 5 to 100 rpm, the reduction ratio of the worm gears connected thereto is 1:15, the sputtering power in magnetron sputtering is 50 to 300 W, and the substrate temperature is 20 to 500° C.