A self-supporting nanofiber membrane and its preparation method and application

The preparation of substrate-free self-supported GaN nanofiber membranes through carbon nanofiber template conversion method solves the problem that GaN nanofiber membranes are difficult to achieve self-support structure in the prior art, and realizes efficient nanofiber membrane preparation, expanding its photoelectricity Applications in the field of devices.

CN116288925BActive Publication Date: 2024-11-26MINDU INNOVATION LAB +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111566119.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-12-20
Publication Date
2024-11-26
Estimated Expiration
2041-12-20

Smart Images

  • Figure CN116288925B_ABST
    Figure CN116288925B_ABST
Patent Text Reader

Abstract

The present application discloses a self-supporting nanofiber membrane and its preparation method and application. The self-supporting nanofiber membrane is a pure GaN nanofiber membrane or a GaN@C nanofiber membrane with a coaxial core-shell structure. The self-supporting nanofiber membrane has an independent self-supporting film structure, which can greatly reduce the production cost and the complexity of subsequent application processing technology, and can fully expand its application in ultraviolet detectors, light-emitting diodes, field effect transistors, lasers, photocatalysis, electrocatalysis and other fields.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to a self-supporting nanofiber membrane and a preparation method and application thereof, belonging to the technical field of semiconductor materials. Background Art

[0002] Gallium nitride (GaN) is a third-generation semiconductor material with a direct bandgap. The bandgap width is about 3.4eV at room temperature, corresponding to a cutoff wavelength of 365nm. It has intrinsic ultraviolet light response performance, so it is widely used in optoelectronic components such as ultraviolet detectors, light-emitting diodes, field-effect transistors and lasers. In particular, LEDs in the blue-green light band have promoted the rapid development of the semiconductor lighting industry, and Japanese scientists Isamu Akasaki, Hiroshi Amano and Shuji Nakamura won the 2014 Nobel Prize in Physics for this. In addition, GaN also has excellent electrical properties such as high electrical breakdown strength and high thermal conductivity, so it has recently been used in high-frequency, high-voltage, and high-power electronic components (such as fast charging chargers, adapters, etc.).

[0003] At present, GaN is mainly grown on silicon wafers or sapphire substrates by metal organic vapor deposition (MOCVD) or molecular beam epitaxy (MBE). On the one hand, these methods are complex and require expensive equipment; on the other hand, they require the use of high-quality single crystal epitaxial substrates, and there are problems such as lattice mismatch leading to defects, which limits the preparation and application of GaN materials. In recent years, GaN nanomaterials, especially one-dimensional nanostructures (nanorods, nanotubes, nanowires, etc.) have received widespread attention; due to their high aspect ratio and high specific surface area, they have shown unique advantages in ultraviolet detectors, light-emitting diodes, field effect transistors, lasers, photocatalysis, electrocatalysis and other fields. For example, Professor Fan Shoushan of Tsinghua University used carbon nanotubes as templates to prepare GaN nanorods with a diameter of 4 to 50 nanometers and a length of about 25 microns, and studied their photoluminescence properties (Science, 1997, 277, 1287). Peidong Yang et al. from the University of California, Berkeley, used ZnO nanorods as templates, deposited GaN by high-temperature molecular beam epitaxy, and removed the ZnO template to prepare GaN nanotube arrays with an inner diameter of 30 to 200 nanometers and a wall thickness of 5 to 50 nanometers (Nature, 2003, 422, 599). Although these one-dimensional GaN nanostructures have a large aspect ratio and high specific surface area, most of them are prepared by high-temperature chemical vapor deposition and other methods, which have complex processing techniques and require the use of catalysts; in addition, their length is limited and it is difficult to achieve a macroscopically continuous scale, so they are still loaded on substrates for application.

[0004] Electrospinning is a technique that can prepare continuous-length nanofibers. The diameter of the prepared fibers is usually tens to hundreds of nanometers. The obtained nanofiber membrane has the advantages of light weight, high porosity, and large specific surface area. Generally, polymer nanofiber membranes can be obtained by directly electrospinning polymer solutions, and carbon nanofibers or inorganic nanofibers can be obtained by post-processing related electrospinning precursors. Therefore, researchers have tried to prepare GaN nanofibers by electrospinning technology. For example, Wu et al. tried to use PVP as a spinning aid and template, add gallium nitrate (Ga(NO3)3) for spinning, and obtain PVP / Ga(NO3)3 nanofiber membranes, and then calcine in air to remove the PVP template, and obtain polycrystalline GaN nanofibers by ammonia nitridation (Adv. Mater., 2009, 21, 227). Although the prepared GaN nanofibers show a one-dimensional fiber structure at the microscopic level, they are still powdery at the macroscopic level and are not self-supporting fiber membrane structures, which limits their application.

[0005] In summary, one-dimensional GaN nanofibers have the advantages of high aspect ratio and high specific surface area, and have unique advantages in the application fields of optoelectronic devices, etc. However, the preparation of GaN nanofiber membranes with substrate-free self-supporting structures is still very challenging. Therefore, this patent discloses a carbon nanofiber template conversion method to prepare self-supporting GaN nanofiber membranes. Summary of the invention

[0006] According to one aspect of the present application, a self-supporting nanofiber membrane is provided, wherein the self-supporting nanofiber membrane is a pure GaN nanofiber membrane or a GaN@C nanofiber membrane with a coaxial core-shell structure. The self-supporting nanofiber membrane has an independent self-supporting film structure, which can greatly reduce production costs and the complexity of subsequent application processing technology, and can fully expand its application in ultraviolet detectors, light-emitting diodes, field effect transistors, lasers, photocatalysis, electrocatalysis and other fields.

[0007] A self-supporting nanofiber membrane is a pure GaN nanofiber membrane or a GaN@C nanofiber membrane with a coaxial core-shell structure.

[0008] The self-supporting nanofiber membrane is a substrate-free self-supporting nanofiber membrane.

[0009] Optionally, the fibers in the self-supporting nanofibrous membrane have a one-dimensional continuous nanostructure.

[0010] Optionally, the fiber diameter in the self-supporting nanofiber membrane is 50 to 1000 nanometers.

[0011] Optionally, the fiber diameter in the self-supporting nanofiber membrane is a range value formed between any two values ​​of 50, 100, 200, 400, 500, 600, 700, 900, 1000 nanometers.

[0012] Optionally, the self-supporting nanofiber membrane has a thickness of 10 to 100 microns.

[0013] Optionally, the thickness of the self-supporting nanofiber membrane is any one of 10, 20, 30, 40, 50, 60, 70, 80, 90, 100 microns or a range formed between any two values.

[0014] Optionally, the self-supporting nanofiber membrane has a porous network structure with a porosity of 65-90%.

[0015] Optionally, the specific surface area of ​​the self-supporting nanofiber membrane is 50 to 300 m 2 / g.

[0016] Optionally, the self-supporting nanofibrous membrane has a hexagonal wurtzite structure.

[0017] According to another aspect of the present application, a method for preparing the self-supporting nanofiber membrane described in any one of the above is provided, the preparation method comprising the following steps:

[0018] The carbon nanofiber membrane is used as a sacrificial template and converted in a raw material containing gallium, gallium oxide and ammonia to obtain the self-supporting nanofiber membrane.

[0019] Optionally, the fiber diameter of the carbon nanofiber membrane is 50 to 1000 nanometers.

[0020] Optionally, the fiber diameter of the carbon nanofiber membrane is a range value formed between any two values ​​of 50, 100, 200, 400, 500, 600, 700, 900, and 1000 nanometers.

[0021] Preferably, the carbon nanofiber membrane has a thickness of 10 to 100 microns.

[0022] Optionally, the carbon content of the carbon nanofiber membrane is 90 wt % or more.

[0023] Optionally, the carbon nanofiber membrane is selected from at least one of a non-oriented carbon nanofiber membrane and an oriented carbon nanofiber membrane.

[0024] Optionally, the preparation method comprises the following steps:

[0025] (S1) obtaining a self-supporting carbon nanofiber membrane;

[0026] (S2) covering the mixture with a self-supporting carbon nanofiber membrane, heating it in an ammonia atmosphere, and reacting it to obtain the self-supporting nanofiber membrane;

[0027] The mixture contains gallium and gallium oxide.

[0028] Optionally, the (S1) is:

[0029] (S1-1) obtaining a polymer precursor nanofiber membrane;

[0030] (S1-2) heat-treating the polymer precursor nanofiber membrane at high temperature to obtain the carbon nanofiber membrane.

[0031] Optionally, in (S1-1), the polymer in the polymer precursor nanofiber membrane includes at least one of polyacrylonitrile, polyimide, polyamide, polyvinyl alcohol, polyvinylidene fluoride, polypyrrolone, and polyphenylene.

[0032] Optionally, the polymer precursor nanofiber membrane is obtained by any one of electrospinning, melt blowing, centrifugal spinning, air spinning, and air electrospinning.

[0033] Optionally, the electrospinning conditions include: voltage 15-40 kV; spinning solution supply rate 0.5-3.0 mL / h; the distance between the roller surface and the needle tip is 10-40 cm, the roller speed is 50-2000 rpm; the spinning solution volume is 5.0-20 mL.

[0034] Optionally, in (S1-2), the high temperature treatment includes pre-oxidation at 150-400°C and / or carbonization treatment at 600-1800°C.

[0035] Optionally, the pre-oxidation time is 1.0 to 5.0 h.

[0036] Optionally, the carbonization treatment time is 1.0 to 3.0 hours.

[0037] Optionally, in (S2), the molar ratio of gallium to gallium oxide in the mixture is 1:1 to 10:1.

[0038] Optionally, in (S2), the molar ratio of gallium to gallium oxide in the mixture is any one of 1:1, 1:3, 1:5, 1:7, 1:9, 1:10 or a range formed between any two values.

[0039] Optionally, in (S2), the ammonia flow rate is 10 to 100 cm 3 / min.

[0040] Optionally, in (S2), the ammonia flow rate is 10, 20, 30, 40, 50, 60, 70, 80, 90, 100 cm 3 / min, or the range formed by any two values.

[0041] Optionally, in (S2), the heating rate is 1.0 to 10.0°C / min.

[0042] Optionally, in (S2), the heating rate is any one of 1, 3, 5, 7, 9, 10°C / min or a range formed between any two values.

[0043] Optionally, in (S2), the reaction temperature is 800-1100°C.

[0044] Optionally, in (S2), the reaction temperature is any one of 800, 850, 900, 950, 1000, 1050, 1100°C or a range formed between any two values.

[0045] Optionally, in (S2), the reaction maintenance time t is 10 min to 3.0 h.

[0046] Optionally, in (S2), the reaction maintenance time t is any one of 10 min, 30 min, 50 min, 1 h, 2 h, 3 h, or a range value formed between any two values.

[0047] Preferably, when the self-supporting nanofiber membrane is a pure GaN nanofiber membrane, the reaction maintenance time t is 1.0<t≤3h;

[0048] Preferably, when the self-supporting nanofiber membrane is a GaN@C nanofiber membrane with a coaxial core-shell structure, the reaction maintenance time t is 10 min≤t≤1.0 h.

[0049] According to one aspect of the present application, there is provided an application of the self-supporting nanofiber membrane described in any one of the above items or the self-supporting nanofiber membrane prepared according to any one of the preparation methods described in the above items in the preparation of at least one of ultraviolet detectors, light-emitting diodes, field effect transistors, lasers, photocatalysts, and electrocatalysts.

[0050] As an implementation scheme, the present application discloses a template conversion method for preparing a self-supporting gallium nitride (GaN) nanofiber membrane, which includes: firstly preparing a polymer-based nanofiber membrane (or non-woven fabric, woven fabric) by textile technology such as electrospinning (or melt-blowing, centrifugal spinning, air spinning, gas electrospinning), and obtaining a self-supporting carbon nanofiber membrane by high-temperature heat treatment; then placing the prepared self-supporting carbon nanofiber membrane in a high-temperature furnace, applying a (Ga+Ga2O3) mixed raw material and NH3 gas atmosphere, maintaining a certain reaction temperature, raw material ratio, gas flow rate and reaction time, etc., so that the carbon nanofiber is converted into a GaN nanofiber, and after cooling, a substrate-free self-supporting GaN nanofiber membrane is obtained. The GaN nanofiber of the present invention has the characteristics of a one-dimensional continuous nanostructure, a small fiber diameter, and a high aspect ratio, and its nanofiber membrane has the characteristics of a porous mesh structure, a high porosity, a high specific surface area and self-support. The self-supporting GaN nanofiber membrane is expected to be used in the fields of ultraviolet detectors, light-emitting diodes, field effect transistors, lasers, photocatalysis, electrocatalysis, etc.

[0051] As an embodiment, the present application provides a method for preparing a self-supporting gallium nitride (GaN) nanofiber membrane, using a carbon nanofiber membrane as a sacrificial template, and in a high-temperature furnace, using liquid gallium (Ga) and gallium oxide (Ga2O3) powder as raw materials, converting them into GaN nanofiber membranes at high temperature in an ammonia atmosphere.

[0052] Optionally, the fiber diameter is 50 to 1000 nanometers, and the carbon content is above 90%; it can be a disordered non-oriented nanofiber membrane or non-woven fabric, or an oriented nanofiber membrane, woven fabric, etc.

[0053] Alternatively, the polymer precursor nanofiber membrane can be prepared by electrospinning technology (but not limited to), and then obtained by high temperature heat treatment.

[0054] Optionally, the polymer precursor includes but is not limited to polyacrylonitrile, polyimide, polyamide, polyvinyl alcohol, polyvinylidene fluoride, polypyrrolidone, polyphenylene, etc.; the high-temperature heat treatment process includes pre-oxidation (150-400°C) and / or carbonization treatment (600-1800°C), etc.

[0055] Optionally, the raw material mixing ratio is 1:1 to 10:1 (molar ratio), and the mixed raw materials are placed in a corundum ark; the carbon nanofiber membrane covers the raw material mixture.

[0056] Optionally, it can be a quartz tube furnace or an alumina high temperature ceramic tube furnace, etc., which should have good air tightness, can be vacuumed, and be equipped with a gas flow control valve and a gas flow meter.

[0057] Optionally, the carbon nanofiber membrane and (Ga+Ga2O3) raw materials are placed in a tubular furnace, evacuated and replaced with ammonia several times to remove the air, and then the ammonia atmosphere is maintained, the temperature is raised to a certain temperature and maintained for a certain time, and the GaN nanofiber membrane is obtained after cooling.

[0058] Optionally, the ammonia flow rate is 10 to 100 cm 3 / min, the heating rate is 1.0~10.0℃ / min, the reaction temperature is 800~1100℃, and the reaction maintenance time is 10min~3.0h.

[0059] Optionally, the carbon nanofibers can be completely converted to obtain a pure GaN nanofiber membrane, or the carbon nanofibers can be partially converted to obtain a GaN@C nanofiber membrane with a coaxial core-shell structure.

[0060] Optionally, the fiber diameter is adjustable within the range of 50 to 1000 nanometers, the fiber membrane thickness is adjustable within the fiber within the range of 10 to 100 microns, and the fiber membrane size is determined according to actual application requirements and the size of the tubular furnace, and is not limited by the implementation cases of this patent.

[0061] Optionally, it has the advantages of substrate-free self-supporting properties, porous network structure, high porosity, high specific surface area, etc.

[0062] Optionally, it can be used in the fields of ultraviolet detectors, light-emitting diodes, field-effect transistors, lasers, photocatalysis, electrocatalysis, etc.

[0063] The present application relates to the preparation and application fields of third-generation semiconductor gallium nitride materials, and in particular to the preparation and optoelectronic application fields of one-dimensional gallium nitride nanofiber materials.

[0064] The purpose of this application is to provide a new technical route to prepare GaN fiber materials with one-dimensional nanostructures and develop a substrate-free self-supporting GaN nanofiber membrane.

[0065] The characteristics of this application are that, on the one hand, it overcomes the limitation that the traditional epitaxial growth method needs to use a high-quality substrate to prepare GaN thin films; on the other hand, compared with the reported one-dimensional materials such as GaN nanowires / nanotubes / nanorods, the GaN nanofibers prepared by this invention have a continuous length and a higher aspect ratio, and the nanofiber membrane has the advantages of light weight, high porosity, and high specific surface area. In addition, unlike the above-mentioned electrospinning precursor and heat treatment conversion method, which can only obtain GaN nanofibers that are macroscopically powdered, the GaN nanofiber membrane prepared by the present invention has an independent self-supporting film structure. Therefore, the self-supporting GaN nanofiber membrane can greatly reduce the production cost, reduce the complexity of subsequent application processing technology, and can fully expand its application in the fields of ultraviolet detectors, light-emitting diodes, field-effect transistors, lasers, photocatalysis, electrocatalysis, etc.

[0066] As an embodiment, the preparation method provided in the present application specifically comprises the following steps:

[0067] (1) preparing polymer nanofiber membranes by spinning / spinning techniques such as electrospinning, and obtaining self-supporting carbon nanofiber membranes by high-temperature heat treatment;

[0068] (2) mixing liquid gallium (Ga) and gallium oxide (Ga2O3) powder raw materials, placing them in a corundum ark, and then placing the carbon nanofiber membrane prepared in step (1) into the corundum ark (covering the mixed raw materials);

[0069] (3) placing the corundum ark containing the (Ga+Ga2O3) raw material and the carbon nanofiber membrane in step (2) in the core heating zone of the tubular furnace; evacuating the vacuum and introducing ammonia gas, repeating the process several times to fully remove the air;

[0070] (4) heating the tube furnace to a certain set temperature at a certain heating rate, and maintaining the temperature for a certain period of time after reaching the set temperature, and during the heating and temperature-maintaining process, ammonia gas is continuously introduced to maintain the ammonia reaction atmosphere;

[0071] (5) After natural cooling, a self-supporting GaN nanofiber membrane is obtained.

[0072] In this application, carbon nanofibers are used as sacrificial templates to be converted into GaN nanofibers. The schematic diagram of the conversion process is shown in FIG. Figure 1 shown.

[0073] In the present invention, carbon nanofibers are used as sacrificial templates to be converted into GaN nanofibers, and the chemical reaction that occurs is:

[0074] 4Ga(l)+Ga2O3(s)=3Ga2O(g) (1)

[0075] 2Ga2O(g)+C(s)+4NH3(g)=4GaN(s)+H2O(g)+CO(g)+5H2(g) (2)

[0076] The spinning / textile technology described in step (1) includes, but is not limited to, electrospinning technology, such as melt-blowing, centrifugal spinning, air-spinning, and air-electrospinning. Preferably, the embodiment of the present invention adopts electrospinning technology.

[0077] The polymer described in step (1) is a high molecular material that can be carbonized at high temperature and has a certain carbon residue rate, including but not limited to polyacrylonitrile (PAN), such as polyimide (PI), polyamide (PAI), polyvinyl alcohol (PVA), polyvinylidene fluoride (PVDF), polypyrrolidone (BBB), polyphenylene (PPP), etc. In the embodiment of the present invention, polyacrylonitrile is preferably used.

[0078] The high temperature heat treatment procedure described in step (1) includes pre-oxidation and / or carbonization processes, etc., and the pre-oxidation temperature ranges from 150 to 400°C, and the carbonization temperature ranges from 600 to 1800°C.

[0079] The nanofiber membrane described in step (1) can be a non-oriented nanofiber membrane, non-woven fabric, or an oriented fiber membrane, woven fabric, etc. Preferably, the embodiment of the present invention adopts electrospinning technology to prepare the non-oriented nanofiber membrane.

[0080] The fiber diameter of the carbon nanofiber membrane in step (1) is adjustable within the range of 50 to 1000 nanometers.

[0081] In step (2), the mixing ratio of liquid gallium (Ga) and gallium oxide (Ga2O3) powder raw materials is Ga:Ga2O3=1:1~10:1 (molar ratio); preferably, the ratio is: 4:1.

[0082] The size of the carbon nanofiber membrane in step (2) can be cut according to demand, and is usually smaller than the size of the corundum ark.

[0083] The tube furnace can be a quartz tube furnace or an alumina high temperature ceramic tube furnace, etc. It should have good air tightness, can be vacuumed, and be equipped with a gas flow control valve and a gas flow meter.

[0084] The heating rate in step (4) is 1.0-10.0°C / min; the reaction temperature is set to 800-1100°C; the constant temperature time is 10min-3.0h; the flow rate of ammonia is 10-100cm 3 / min.

[0085] The GaN nanofiber preparation method provided in the present application can effectively obtain GaN nanofibers with one-dimensional continuous size, which have the advantages of small fiber diameter, high specific surface area, high porosity, etc.; in particular, it can effectively obtain substrate-free independent self-supporting GaN nanofiber membranes.

[0086] The GaN nanofibers prepared in the present application have great practical value and can be effectively applied to ultraviolet detectors, light-emitting diodes, field-effect transistors, lasers, photocatalysis, electrocatalysis and other fields.

[0087] The beneficial effects of this application include:

[0088] (1) The self-supporting nanofiber membrane provided in the present application is a pure GaN nanofiber membrane or a GaN@C nanofiber membrane with a coaxial core-shell structure, and has an independent self-supporting film structure. It can greatly reduce the production cost and the complexity of subsequent application processing technology, and can fully expand its application in the fields of ultraviolet detectors, light-emitting diodes, field effect transistors, lasers, photocatalysis, electrocatalysis, etc.

[0089] (2) The method for preparing a self-supporting nanofiber membrane provided in the present application uses a carbon nanofiber membrane as a sacrificial template. In a high-temperature furnace, liquid gallium (Ga) and gallium oxide (Ga2O3) powder are used as raw materials and converted into a GaN nanofiber membrane at high temperature in an ammonia atmosphere to obtain a pure GaN nanofiber membrane or a GaN@C nanofiber membrane with a coaxial core-shell structure. The membrane has an independent self-supporting film structure. Not only does the obtained self-supporting nanofiber membrane have excellent performance, but it also overcomes the limitation that the traditional epitaxial growth method for preparing GaN thin films requires the use of high-quality substrates. BRIEF DESCRIPTION OF THE DRAWINGS

[0090] Figure 1 Schematic diagram of the process of converting a carbon nanofiber membrane as a sacrificial template into a self-supporting GaN nanofiber membrane in this application.

[0091] Figure 2 a is a physical picture of the self-supporting carbon nanofiber membrane prepared in step (1) of Example 1 of the present application; Figure 2 b is a scanning electron microscope image of the self-supporting carbon nanofiber membrane prepared in step (1) of Example 1 of the present application.

[0092] Figure 3 a is the X-ray diffraction spectrum (XRD) of the carbon nanofiber membrane prepared in step (1) of Example 1 of the present application; Figure 3 b is the Raman spectrum (Raman) of the carbon nanofiber membrane prepared in step (1) of Example 1 of the present application.

[0093] Figure 4 This is a physical picture of the self-supporting GaN@C nanofiber membrane prepared in step (2) of Example 1 of the present application.

[0094] Figure 5 This is a scanning electron microscope image of the self-supporting GaN@C nanofiber membrane prepared in step (2) of Example 1 of the present application (a is the surface; b is the cross section).

[0095] Figure 6 This is the X-ray diffraction spectrum (XRD) of the self-supporting GaN@C nanofiber membrane prepared in step (2) of Example 1 of the present application.

[0096] Figure 7 This is a physical picture of the self-supporting pure GaN nanofiber membrane prepared in step (2) of Example 2 of the present application.

[0097] Figure 8 This is a scanning electron microscope image of the self-supporting GaN nanofiber membrane prepared in step (2) of Example 2 of the present application (a is the surface; b is a local magnified image).

[0098] Fig. 9This is the X-ray diffraction spectrum (XRD) of the self-supporting GaN nanofiber membrane prepared in step (2) of Example 2 of the present application. DETAILED DESCRIPTION

[0099] The present application is described in detail below with reference to embodiments, but the present application is not limited to these embodiments.

[0100] Unless otherwise specified, the raw materials in the examples of this application were purchased through commercial channels.

[0101] Description of materials / reagents used in the examples:

[0102] Polyacrylonitrile (PAN), molecular weight (M w ) is 150,000, Sigma-Aldrich.

[0103] Gallium metal (Ga), 99.99%, Shanghai Aladdin Biochemical Technology Co., Ltd.

[0104] Gallium oxide (Ga2O3), 99.99%, Shanghai Aladdin Biochemical Technology Co., Ltd.

[0105] Ammonia (NH3), ≥99.999%, Fuzhou Huaxinda Industrial Gas Co., Ltd.

[0106] The schematic diagram of the process of converting the carbon nanofiber membrane into a self-supporting GaN / GaN@C nanofiber membrane using a sacrificial template in this application is shown in Figure 1 shown.

[0107] Example 1: Preparation of coaxial core-shell GaN@C nanofiber membrane

[0108] (1) Preparation of self-supporting carbon nanofiber membranes

[0109] In this embodiment, polyacrylonitrile (PAN) is selected as a polymer precursor, and a PAN nanofiber membrane is prepared by electrospinning technology, and a carbon nanofiber membrane is obtained by pre-oxidation and carbonization. The specific steps are as follows:

[0110] (1-1) Preparation of PAN spinning solution: PAN powder (M w =150,000) was added into DMF solvent, heated and stirred to obtain a PAN solution with a concentration of 10 wt%;

[0111] (1-2) PAN nanofiber membrane was prepared by electrospinning technology. The electrospinning conditions were as follows: voltage 20 kV; spinning solution supply rate 1.5 mL / h; the receiving device was a rotating drum, the distance between the drum surface and the needle tip was about 25 cm, and the drum speed was about 50 rpm; the spinning solution volume was 10 mL. (Note: the fiber diameter can be adjusted by adjusting the voltage, spinning solution supply rate and receiving distance; the fiber membrane thickness can be adjusted by adjusting the amount of spinning solution). After the electrospinning was completed, the fiber membrane was peeled off the drum to obtain a non-oriented PAN nanofiber membrane.

[0112] (1-3) Pre-oxidation treatment: The PAN nanofiber membrane prepared in step (1-2) was cut into small pieces (about 5 cm*10 cm), placed in a tubular furnace, heated to 250°C at a heating rate of 5°C / min in an air atmosphere, and then maintained at 250°C for 3 hours.

[0113] (1-4) Carbonization treatment: The PAN nanofiber membrane pre-oxidized in step (1-3) was sandwiched between graphite plates, placed in a quartz tube furnace, heated to 1000°C at a heating rate of 5°C / min in an argon atmosphere, and then maintained at 1000°C for 1 hour; after cooling, a self-supporting carbon nanofiber membrane was obtained.

[0114] The obtained carbon nanofiber membrane performance: The obtained carbon nanofiber membrane is a non-oriented nanofiber membrane, the fiber membrane thickness is about 50 microns, the fiber diameter is about 500 nanometers, the carbon content is greater than 95wt%, and it has a self-supporting structure and can be bent and folded.

[0115] Figure 2 a is a physical picture of the self-supporting carbon nanofiber membrane prepared in step (1); Figure 2 b is a scanning electron microscope image of the self-supporting carbon nanofiber membrane prepared in step (1), indicating that the prepared carbon nanofiber membrane has a self-supporting structure and good flexibility, and can be bent without breaking; the surface of the nanofiber is smooth, and the fiber diameter is evenly distributed, about 500 nanometers.

[0116] Figure 3 a is the X-ray diffraction spectrum (XRD) of the carbon nanofiber membrane prepared in step (1); Figure 3 b is the Raman spectrum of the carbon nanofiber membrane prepared in step (1), indicating that the prepared carbon nanofiber membrane has a typical carbon material structure and a certain crystalline structure.

[0117] (2) Preparation of self-supporting gallium nitride@carbon (GaN@C) core-shell nanofiber membranes

[0118] The carbon nanofibers prepared in step (1) are used as sacrificial templates and converted into GaN@C nanofiber membranes through high-temperature chemical reactions. The specific steps are as follows:

[0119] (2-1) 2.79 g of liquid gallium and 1.87 g of gallium oxide (molar ratio of 4:1) were mixed evenly and placed in a corundum ark, and a piece of carbon nanofiber membrane was placed on the mixed raw materials.

[0120] (2-2) Place the corundum ark prepared in step (1) in a quartz tube furnace; first evacuate the furnace to remove air, then introduce ammonia gas, and repeat this process 3 times.

[0121] (2-3) Heating to 900°C at a heating rate of 5°C / min, and then maintaining the temperature at 900°C for 1 hour; during this process, the ammonia atmosphere was maintained, and the ammonia flow rate was 50 cm 3 / min.

[0122] (2-4) After cooling to room temperature, a self-supporting GaN@C core-shell nanofiber membrane was obtained.

[0123] The obtained GaN@C nanofiber membrane has the following properties: the nanofiber diameter is about 500-600 nanometers; the XRD diffraction peak shows that GaN has a hexagonal wurtzite structure with residual carbon; the GaN@C nanofiber membrane has a self-supporting structure, a thickness of about 60 microns, a porosity of 85%, and a surface area of ​​250 cm 2 / g.

[0124] Figure 4 This is a physical picture of the self-supporting GaN@C nanofiber membrane prepared in step (2).

[0125] Figure 5 This is a scanning electron microscope image of the self-supporting GaN@C nanofiber membrane prepared in step (2) (a is the surface; b is the cross-section), indicating that GaN@C has a continuous one-dimensional fiber structure, the fiber surface is rough, and the fiber diameter is about 500 to 600 nanometers; the cross-sectional scanning electron microscope image clearly shows a coaxial core-shell structure: the outer layer of the fiber is GaN, and the inner core is residual (incompletely converted) carbon nanofibers.

[0126] Figure 6 The X-ray diffraction spectrum (XRD) of the self-supporting GaN@C nanofiber membrane prepared in step (2) shows that the GaN nanofiber is successfully prepared, its structure is a hexagonal wurtzite structure, and the residual carbon peak can be clearly seen.

[0127] Example 2: Preparation of pure GaN nanofiber membrane

[0128] (1) Preparation of self-supporting carbon nanofiber membranes

[0129] The method and steps are the same as in Example 1.

[0130] (2) Preparation of self-supporting pure GaN nanofiber membrane

[0131] The carbon nanofibers prepared in step (1) are used as sacrificial templates and converted into GaN nanofiber membranes through high-temperature chemical reactions. The specific steps are as follows:

[0132] (2-1) 2.79 g of liquid gallium and 1.87 g of gallium oxide (molar ratio of 4:1) were mixed evenly and placed in a corundum ark, and a piece of carbon nanofiber membrane was placed on the mixed raw materials.

[0133] (2-2) Place the corundum ark prepared in step (1) in a quartz tube furnace; first evacuate the furnace to remove air, then introduce ammonia gas, and repeat this process 3 times.

[0134] (2-3) Heating to 1000°C at a heating rate of 5°C / min, and then maintaining the temperature at 1000°C for 2 hours; during this process, the ammonia atmosphere was maintained, and the ammonia flow rate was 50 cm 3 / min.

[0135] (2-4) After cooling to room temperature, a self-supporting GaN nanofiber membrane was obtained.

[0136] The obtained GaN@C nanofiber membrane has the following properties: the nanofiber diameter is about 900-1000 nanometers, the XRD diffraction peak shows that GaN has a hexagonal wurtzite structure, the GaN nanofiber membrane has a self-supporting structure, the thickness is about 80 microns, the porosity is 70%, and the specific surface area is 300 cm 2 / g.

[0137] Figure 7 This is a physical picture of the self-supporting pure GaN nanofiber membrane prepared in step (2).

[0138] Figure 8 This is a scanning electron microscope image of the self-supporting GaN nanofiber membrane prepared in step (2) (a is the surface; b is a local magnified image), which shows that GaN has a continuous one-dimensional fiber structure, the fiber surface is rough, and there is adhesion between the fibers. The fiber diameter is about 900 to 1000 nanometers.

[0139] Fig. 9 The X-ray diffraction spectrum (XRD) of the self-supporting GaN nanofiber film prepared in step (2) shows that the GaN nanofiber is successfully prepared, its structure is a hexagonal wurtzite structure, and no residual carbon peak is observed.

[0140] The above are only a few embodiments of the present application and do not constitute any form of limitation to the present application. Although the present application is disclosed as above with preferred embodiments, it is not intended to limit the present application. Any technician familiar with the profession, without departing from the scope of the technical solution of the present application, using the technical content disclosed above to make slight changes or modifications are equivalent to equivalent implementation cases and fall within the scope of the technical solution.

Claims

1. A self-supporting nanofiber membrane, It is characterized in that The self-supporting nanofiber membrane is a pure GaN nanofiber membrane or a GaN@C nanofiber membrane with a coaxial core-shell structure; The self-supporting nanofiber membrane has a porous network structure with a porosity of 65-90%; The specific surface area of ​​the self-supporting nanofiber membrane is 50-300 m 2 / g; (1) preparing polymer nanofiber membranes by electrospinning / spinning technology and obtaining self-supporting carbon nanofiber membranes by heat treatment; (2) mixing liquid gallium and gallium oxide powder raw materials, placing them in a corundum ark, and then placing the self-supporting carbon nanofiber membrane prepared in step (1) in the corundum ark to cover the mixed raw materials; (3) placing the corundum ark containing the liquid gallium and gallium oxide powder raw materials and the self-supporting carbon nanofiber membrane in step (2) in the core heating zone of the tube furnace, evacuating the chamber and introducing ammonia gas, and repeating the process several times to fully remove the air; (4) heating the tube furnace to a set temperature and then maintaining the temperature, and continuously introducing ammonia gas during the heating and temperature-maintaining process to maintain an ammonia reaction atmosphere; (5) After natural cooling, a self-supporting nanofiber membrane is obtained.

2. The self-supporting nanofiber membrane according to claim 1, It is characterized in that The fibers in the self-supporting nanofiber membrane have a one-dimensional continuous nanostructure.

3. The self-supporting nanofiber membrane according to claim 1, It is characterized in that The fiber diameter in the self-supporting nanofiber membrane is 50 to 1000 nanometers.

4. The self-supporting nanofiber membrane according to claim 1, It is characterized in that The thickness of the self-supporting nanofiber membrane is 10 to 100 microns.

5. The self-supporting nanofiber membrane according to claim 1, It is characterized in that The self-supporting nanofiber membrane has a hexagonal wurtzite structure.

6. The method for preparing the self-supporting nanofiber membrane according to any one of claims 1 to 5, It is characterized in that The preparation method comprises the following steps: The carbon nanofiber membrane is used as a sacrificial template and converted in a raw material containing gallium, gallium oxide and ammonia to obtain the self-supporting nanofiber membrane.

7. The preparation method according to claim 6, It is characterized in that The fiber diameter of the carbon nanofiber membrane is 50-1000 nanometers.

8. The preparation method according to claim 6, It is characterized in that The thickness of the carbon nanofiber membrane is 10-100 microns.

9. The preparation method according to claim 6, It is characterized in that The carbon content of the carbon nanofiber membrane is 90wt% or more.

10. The preparation method according to claim 6, It is characterized in that The carbon nanofiber membrane is selected from at least one of a non-oriented carbon nanofiber membrane and an oriented carbon nanofiber membrane.

11. The preparation method according to claim 6, It is characterized in that The preparation method comprises the following steps: (S1) Obtaining a self-supporting carbon nanofiber membrane; (S2) covering the mixture with a self-supporting carbon nanofiber membrane, heating the mixture in an ammonia atmosphere, and reacting the mixture to obtain the self-supporting nanofiber membrane; The mixture contains gallium and gallium oxide.

12. The preparation method according to claim 11, It is characterized in that In (S2), the molar ratio of gallium to gallium oxide in the mixture is 1:1 to 10:

1.

13. The preparation method according to claim 11, It is characterized in that (S2) The ammonia flow rate is 10~100cm 3 / min.

14. The preparation method according to claim 11, It is characterized in that In (S2), the heating rate is 1.0~10.0℃ / min.

15. The preparation method according to claim 11, It is characterized in that In (S2), the reaction temperature is 800~1100℃.

16. The preparation method according to claim 11, It is characterized in that In (S2), the reaction maintenance time t is 10min~3.0h.

17. The preparation method according to claim 11, It is characterized in that When the self-supporting nanofiber membrane is a pure GaN nanofiber membrane, the reaction maintenance time t is 1.0h<t≤3h.

18. The preparation method according to claim 11, It is characterized in that When the self-supporting nanofiber membrane is a GaN@C nanofiber membrane with a coaxial core-shell structure, the reaction maintenance time t is 10min≤t≤1.0h.

19. The self-supporting nanofiber membrane according to any one of claims 1 to 5 or the self-supporting nanofiber membrane prepared by the preparation method according to any one of claims 6 to 18 is used in at least one of the preparation of ultraviolet detectors, light-emitting diodes, field effect transistors, lasers, photocatalysts, and electrocatalysts.