A wave-absorbing nonwoven fabric

By combining chemical fiber base materials and vegetation camouflage materials in absorbing non-woven fabrics, the problems of poor adhesion and lack of camouflage function of existing absorbing materials are solved, and efficient electromagnetic wave absorption and camouflage effects in multiple frequency bands are achieved, which is suitable for Military stealth applications.

CN116288933BActive Publication Date: 2024-10-08SHIJIAZHUANG PANJIANG TECH CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310349129.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-04-04
Publication Date
2024-10-08
Estimated Expiration
2043-04-04

AI Technical Summary

Technical Problem

Existing absorbing materials have poor adhesion, high absorber density, narrow absorption band, easy oxidation and shedding, difficulty in maintenance, and lack of camouflage function. They cannot effectively cope with multi-spectrum reconnaissance methods, resulting in the invisibility of protecting military facilities in military applications. The effect is not ideal enough.

Method used

A kind of absorbing non-woven fabric is used. The formula includes chemical fiber base material, mixed metal powder and vegetation camouflage material. By controlling the formula proportion and process steps, a material that can efficiently absorb electromagnetic waves in multiple frequency bands and imitate the electromagnetic wave reflectivity of plants is prepared. Achieve camouflage effect.

Benefits of technology

It achieves strong electromagnetic wave absorption rate for each main frequency band of radar, and achieves a more realistic camouflage effect through vegetation camouflage imitation effect, deceiving reconnaissance parties, and has significant military application prospects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116288933B_ABST
    Figure CN116288933B_ABST
Patent Text Reader

Abstract

A wave-absorbing nonwoven fabric relates to the technical field of electromagnetic wave absorbing materials. The weight parts of the formula raw materials are: 65-75 parts of chemical fiber base material, 10-15 parts of mixed metal powder for wave absorption, 10-15 parts of vegetation camouflage material, 2-3 parts of methyl methacrylate and 2-3 parts of aluminate coupling agent. The electromagnetic wave absorption rate of each main frequency band of radar is strong, and the vegetation camouflage performance can make the nonwoven fabric well imitate the electromagnetic wave reflectivity of plants, and can produce a weaker wave absorption effect than the nonwoven fabric in the area of ​​simulating vegetation, so as to achieve a more realistic camouflage effect, and create the illusion that the area is covered with vegetation for the reconnaissance party. In this way, the reconnaissance party sees that the area has an uneven electromagnetic wave reflectivity similar to that of the natural environment, so as to achieve the purpose of deceiving the radar of the reconnaissance party, and has a good military application prospect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of wave-absorbing materials, and in particular to a wave-absorbing nonwoven fabric. Background Art

[0002] Stealth technology is an effective means to improve the battlefield survivability of military targets, the concealed penetration capability of weapon systems and the overall combat effectiveness of troops. It is an important research direction and key military technology for the development of the national defense system. Major military countries in the world are striving to make their personnel and various types of weapons and equipment stealth. In actual combat, with the rapid development of composite reconnaissance technology and multi-spectrum detection methods, battlefield reconnaissance has gradually expanded from the initial optical detection to multi-spectrum composite reconnaissance combining optics, infrared, radar, laser, and hyperspectral. Correspondingly, the stealth materials that used to be mainly optical camouflage will find it difficult to cope with multi-spectrum reconnaissance methods. The camouflage stealth materials for personnel and weapons and equipment such as tanks, aircraft, and ships will inevitably expand in the direction of multi-band compatibility such as optics, infrared, and radar.

[0003] Currently, most radar wave absorbing materials are made of micro-powder absorbers, which are made through coating or filling processes. They are mostly in the form of hard materials. They mainly have problems such as poor adhesion to the structure, high absorber density, narrow absorption band, easy oxidation and shedding, and difficult maintenance.

[0004] Moreover, although the coating of this kind of absorbent absorbs the electromagnetic waves of the reconnaissance radar to a certain extent, resulting in the reconnaissance party's radar equipment not receiving the reflected radar electromagnetic waves, thereby achieving the purpose of invisibility, the opponent's radar equipment, although unable to receive the reflected radar electromagnetic waves, the radar wave feedback in the regular area covered by the invisible material is consistent. In other words, although the reconnaissance party does not know what outline is hidden there, the reconnaissance party knows that the radar wave feedback between the area covered by the stealth material and the surrounding environment is obviously different. Therefore, it can be determined that there is a high possibility that the area is covered by the stealth material. In this regard, unmanned reconnaissance aircraft can be sent to conduct close reconnaissance of the target area.

[0005] It can be seen from this that although this uniform absorbing material can absorb electromagnetic waves, it lacks radar electromagnetic wave camouflage function and is insufficient for the protection of modern military facilities.

[0006] Non-woven fabrics, also known as non-woven fabrics, needle-punched cotton, needle-punched non-woven fabrics, etc., are made of polyester fiber, polyester fiber (abbreviated as: PET) and are made through a needle-punching process. They can be made into different thicknesses, feels, hardness, etc.

[0007] Non-woven fabric is a kind of fabric that does not require spinning and weaving. It is made by directional or random arrangement of textile short fibers or filaments to form a fiber web structure, and then reinforced by mechanical, thermal bonding or chemical methods.

[0008] In recent years, non-woven fabrics have been used more and more frequently in the field of electromagnetic wave absorbing materials. The invention patent with publication number CN111321588A discloses absorbing materials based on vertical microporous flexible non-woven fabrics and their preparation and application. After the absorbing powder material is prepared into a liquid, the amount of absorbing powder material incorporated in the vertical microporous flexible non-woven fabric can be controlled by controlling the solid content of the absorbing powder in the absorbing powder solution, the time for the vertical microporous flexible non-woven fabric to be immersed in the absorbing powder solution, the liquid carrying rate of the taken out vertical microporous flexible non-woven fabric, etc., thereby controlling the electromagnetic wave absorption rate of the obtained absorbing material, and forming absorbing materials with different electromagnetic wave absorption rates to meet the application requirements of different working conditions.

[0009] The absorbing material of the patented non-woven fabric can have a high absorption rate for electromagnetic waves in a wider frequency band, thereby achieving the purpose of absorbing and stealth. However, it has no camouflage design and cannot meet the purpose of hiding from military target radar. Summary of the invention

[0010] In order to improve the shortcomings of existing absorbing materials, such as poor adhesion to the structure, high absorbent density, narrow absorbing frequency band, easy oxidation and shedding, difficult maintenance, and lack of camouflage, the present invention provides an absorbing nonwoven fabric. The following technical solutions are adopted:

[0011] A wave-absorbing nonwoven fabric has the following raw materials in parts by weight: 65-75 parts of a chemical fiber base material, 10-15 parts of mixed metal powder for wave absorption, 10-15 parts of vegetation camouflage material, 2-3 parts of methyl methacrylate and 2-3 parts of an aluminate coupling agent.

[0012] Optionally, the weight parts of the formula raw materials are: 68-71 parts of chemical fiber base material, 10-13 parts of mixed metal powder for absorbing waves, 10-13 parts of vegetation camouflage material, 2-3 parts of methyl methacrylate and 2-3 parts of aluminate coupling agent.

[0013] Optionally, the formula raw materials include: 67.8 parts by weight of chemical fiber base material, 14.2 parts of mixed metal powder for absorbing waves, 12.2 parts of vegetation camouflage material, 2.5 parts of methyl methacrylate and 2.1 parts of aluminate coupling agent.

[0014] Through the above technical scheme, through the camouflage absorbing non-woven fabric with the above formula, the mixed metal powder can absorb the electromagnetic waves in each main frequency band very well, and the vegetation camouflage material can make the non-woven fabric have a good imitation of the electromagnetic wave reflectivity of plants, which creates the illusion that the area is a vegetation-covered area for the reconnaissance party. In this way, the reconnaissance party sees that the electromagnetic wave reflectivity of this area is uneven, which is similar to the environment, thereby achieving the purpose of deceiving the radar of the reconnaissance party.

[0015] Optionally, the chemical fiber base material is a mixture of polyacrylonitrile and polypropylene fibers, and the weight ratio of the polyacrylonitrile and polypropylene fibers is 1.5:1.

[0016] Through the above technical scheme, by using the above polyacrylonitrile and polypropylene fibers to form the chemical fiber base material, the non-woven fabric has good thermal insulation and waterproof properties while ensuring a certain strength and softness.

[0017] Optionally, the mixed metal powder consists of nickel-iron alloy powder, nickel powder, iron powder and nano-silver powder, and the weight ratio of the nickel-iron alloy powder, nickel powder, iron powder and nano-silver powder is 2:1:1:0.5.

[0018] Through the above technical scheme, by using the above weight proportions of nickel-iron alloy powder, nickel powder, iron powder and nano silver powder and chemical fiber, the manufactured non-woven fabric can effectively absorb a large proportion of electromagnetic waves in different frequency bands.

[0019] Optionally, the particle sizes of the nickel-iron alloy powder, nickel powder and iron powder are all 500-1000 mesh, and the particle size of the nano silver powder is 10-100 nanometers.

[0020] Through the above technical solution, by using the nickel-iron alloy powder, nickel powder and iron powder with the above particle size, and nano silver powder, electromagnetic waves can be better absorbed.

[0021] Optionally, the vegetation camouflage material is made of straw-based plant fibers to simulate leaf veins, Lyocell fibers are filled into the gaps of the straw-based plant fibers, and the weight ratio of the dry sycamore leaf stems to the fibrinolytic agent is 1:(2-3).

[0022] Through the above technical solution, straw-based plant fibers are used as simulated leaf veins, and Lyocell fibers, which are known as the green fibers of the 21st century, are filled to produce simulated leaves that can absorb electromagnetic waves to a certain extent. However, the proportion of electromagnetic waves absorbed is smaller than that of the non-woven fabric itself. Therefore, a more realistic camouflage effect can be achieved, eliminating the suspicion of the reconnaissance party about the obscured camouflaged target.

[0023] A method for preparing a microwave-absorbing nonwoven fabric comprises the following specific steps:

[0024] Step 1: Preparation of chemical fiber base material, add the weight parts of polyacrylonitrile and polypropylene fiber granules into a high-temperature stirring tank, set the temperature to 235-255°C, stir for 5 minutes, and the stirring paddle speed is 90-95rpm, then add the weight parts of nickel-iron alloy powder, nickel powder, iron powder and nano silver powder, set the temperature to 255-265°C, stir for 10-15 minutes to make a molten material for standby use, and the stirring paddle speed is 110-120rpm;

[0025] Step 2: Preparation of vegetation camouflage material, taking the said weight portion of straw-based plant fiber particles and adding them into an extruder equipped with a leaf vein imitation mold, extruding and forming the shape of plant leaf veins at 150-200°C, and then putting them into a leaf pressing mold, dissolving the said weight portion of Lyocell fiber particles in an aqueous solution with a pH value of 8.0-8.7 and a temperature of 70-80°C, and then adding them through the gate of the leaf pressing mold, controlling the temperature of the leaf pressing mold to rise to 110°C, keeping warm for 10 minutes, and demolding and taking out the vegetation camouflage material after the water is dried for use;

[0026] Step 3: Add the molten material prepared in Step 1 to the non-woven fabric production line for melt extrusion, fiber forming, and wire drawing into a web in sequence, and then lay the vegetation camouflage material prepared in Step 2 on the upper surface of the semi-finished non-woven fabric web in a disordered manner. After the laying is completed, the vegetation camouflage material covers 20-40% of the upper surface of the non-woven fabric;

[0027] Step 4: Use the non-woven spunlace process to reinforce the non-woven web semi-finished product and vegetation camouflage material in Step 3 through 2-3 times of needle punching process, and then enter the non-woven hot press for one-time hot pressing. The drum temperature of the non-woven hot press is set to 120-130℃.

[0028] Through the above technical scheme, the non-woven fabric prepared by the above method has a compact structure and can play a good wave-absorbing role. At the same time, it can also imitate vegetation such as leaves on the surface, and can produce a weaker wave-absorbing ability than the non-woven fabric in the area of ​​​​imitation vegetation, thereby achieving a more realistic camouflage effect.

[0029] In summary, the present invention includes at least one of the following beneficial technical effects:

[0030] The present invention provides an absorbing non-woven fabric, which has a strong absorption rate for electromagnetic waves in various main frequency bands of radar. The vegetation camouflage performance enables the non-woven fabric to well imitate the electromagnetic wave reflectivity of plants, and can produce a weaker absorbing effect than the non-woven fabric in the area of ​​imitating vegetation, thereby achieving a more realistic camouflage effect, creating an illusion that the area is a vegetation-covered area for the reconnaissance party, so that the reconnaissance party sees that the area has an uneven electromagnetic wave reflectivity similar to that of a natural environment, thereby achieving the purpose of deceiving the radar of the reconnaissance party, and having a good military application prospect. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Figure 1 is a schematic diagram of radar imaging simulation according to the first embodiment of the present invention;

[0032] Figure 2 It is a schematic diagram of radar imaging simulation according to the third embodiment of the present invention. DETAILED DESCRIPTION

[0033] The present invention is further described in detail below with reference to the embodiments.

[0034] The embodiment of the present invention discloses a microwave-absorbing nonwoven fabric.

[0035] A wave-absorbing nonwoven fabric has the following raw materials in parts by weight: 65-75 parts of a chemical fiber base material, 10-15 parts of mixed metal powder for wave absorption, 10-15 parts of vegetation camouflage material, 2-3 parts of methyl methacrylate and 2-3 parts of an aluminate coupling agent.

[0036] The weight parts of the raw materials in the formula are: 68-71 parts of chemical fiber base material, 10-13 parts of mixed metal powder for absorbing waves, 10-13 parts of vegetation camouflage material, 2-3 parts of methyl methacrylate and 2-3 parts of aluminate coupling agent.

[0037] The weight parts of the raw materials in the formula are: 67.8 parts of chemical fiber base material, 14.2 parts of mixed metal powder for absorbing waves, 12.2 parts of vegetation camouflage material, 2.5 parts of methyl methacrylate and 2.1 parts of aluminate coupling agent.

[0038] The camouflaged absorbing non-woven fabric with the above formula has a strong absorption rate for electromagnetic waves in each main frequency band, and the vegetation camouflage material can make the non-woven fabric have a good imitation of the electromagnetic wave reflectivity of plants, creating the illusion that the area is covered with vegetation to the reconnaissance party. In this way, the reconnaissance party sees that the electromagnetic wave reflectivity of this area is uneven, which is similar to the environment, thereby achieving the purpose of deceiving the reconnaissance party's radar.

[0039] The chemical fiber base material is a mixture of polyacrylonitrile and polypropylene fibers, and the weight ratio of polyacrylonitrile to polypropylene fibers is 1.5:1.

[0040] By adopting the above-mentioned polyacrylonitrile and polypropylene fibers to form the chemical fiber base material, the non-woven fabric has good thermal insulation and waterproof properties while ensuring a certain strength and softness.

[0041] The mixed metal powder consists of nickel-iron alloy powder, nickel powder, iron powder and nano silver powder, and the weight ratio of the nickel-iron alloy powder, nickel powder, iron powder and nano silver powder is 2:1:1:0.5.

[0042] By using the above-mentioned weight proportions of nickel-iron alloy powder, nickel powder, iron powder and nano silver powder with chemical fiber base material, the manufactured non-woven fabric can effectively absorb a large proportion of electromagnetic waves in different frequency bands.

[0043] The particle sizes of the nickel-iron alloy powder, nickel powder and iron powder are all 500-1000 meshes, and the particle size of the nano silver powder is 10-100 nanometers.

[0044] By adopting the nickel-iron alloy powder, nickel powder and iron powder with the above-mentioned particle size, and nano silver powder, electromagnetic waves can be better absorbed.

[0045] The vegetation camouflage material is made of straw-based plant fibers to simulate leaf veins, Lyocell fibers are filled into the gaps of the straw-based plant fibers, and the weight ratio of dry sycamore leaf stems to the fibrinolytic agent is 1:(2-3).

[0046] The simulated leaves made of straw-based plant fibers are filled with Lyocell fibers, which are known as the green fibers of the 21st century. The simulated leaves can absorb electromagnetic waves to a certain extent, but the proportion of electromagnetic waves absorbed is smaller than that of the non-woven fabric itself. Therefore, it can achieve a more realistic camouflage effect and dispel the suspicion of the reconnaissance party about the obscured camouflaged target.

[0047] A method for preparing a microwave-absorbing nonwoven fabric comprises the following specific steps:

[0048] Step 1: Preparation of chemical fiber base material: add parts by weight of polyacrylonitrile and polypropylene fiber granules into a high-temperature stirring tank, set the temperature to 235-255°C, stir for 5 minutes, and rotate the stirring paddle at 90-95rpm. Then add parts by weight of nickel-iron alloy powder, nickel powder, iron powder and nano silver powder, set the temperature to 255-265°C, stir for 10-15 minutes to form a molten material for standby use, and rotate the stirring paddle at 110-120rpm.

[0049] Step 2: Preparation of vegetation camouflage material: add 10 parts by weight of straw-based plant fiber particles into an extruder equipped with a leaf vein imitation mold, extrude at 150-200°C to form a plant leaf vein imitation shape, and then put it into a leaf pressing mold. Dissolve 10 parts by weight of Lyocell fiber particles in an aqueous solution with a pH value of 8.0-8.7 and a temperature of 70-80°C, and then add it through the gate of the leaf pressing mold. Control the temperature of the leaf pressing mold to rise to 110°C, keep it warm for 10 minutes, and then demould and take out the vegetation camouflage material for use after the water is dried;

[0050] Step 3: Add the molten material prepared in Step 1 to the non-woven fabric production line for melt extrusion, fiber forming, and wire drawing into a web in sequence, and then lay the vegetation camouflage material prepared in Step 2 on the upper surface of the semi-finished non-woven fabric web in a disordered manner. After the laying is completed, the vegetation camouflage material covers 20-40% of the upper surface of the non-woven fabric;

[0051] Step 4: Use the non-woven spunlace process to reinforce the non-woven web semi-finished product and vegetation camouflage material in Step 3 through 2-3 times of needle punching process, and then enter the non-woven hot press for one-time hot pressing. The drum temperature of the non-woven hot press is set to 120-130℃.

[0052] The non-woven fabric prepared by the above method has a compact structure and can play a good wave-absorbing role. At the same time, it can also imitate vegetation such as leaves on the surface, and can produce weaker wave-absorbing ability than non-woven fabric in the area of ​​imitating vegetation, thereby achieving a more realistic camouflage effect.

[0053] Embodiment 1 of the present invention:

[0054] The weight parts of the formula raw materials are: 40.7 parts of polyacrylonitrile, 27.1 parts of polypropylene fiber, 6.3 parts of 500 mesh nickel-iron alloy powder, 3.15 parts of 500 mesh nickel powder, 3.15 parts of 500 mesh iron powder, 1.6 parts of 50 nanometer nano silver powder, 3.48 parts of straw-based plant fiber, 8.72 parts of Lyocell fiber, 2.5 parts of methyl methacrylate and 2.1 parts of aluminate coupling agent.

[0055] The following steps are used to manufacture nonwoven fabrics:

[0056] Step 1: Preparation of chemical fiber base material: add parts by weight of polyacrylonitrile and polypropylene fiber granules into a high-temperature stirring tank, set the temperature to 240°C, stir for 5 minutes, and rotate the stirring paddle at 90 rpm. Then add parts by weight of nickel-iron alloy powder, nickel powder, iron powder and nano silver powder, set the temperature to 260°C, stir for 12 minutes to form a molten material for standby use, and rotate the stirring paddle at 110 rpm.

[0057] Step 2: Preparation of vegetation camouflage material: add 10 parts by weight of straw-based plant fiber particles into an extruder equipped with a leaf vein imitation mold, extrude at 175°C to form a plant leaf vein imitation shape, and then put it into a leaf pressing mold. Dissolve 10 parts by weight of Lyocell fiber particles in an aqueous solution with a pH value of 8.5 and a temperature of 75°C, and then add them through the gate of the leaf pressing mold. Control the temperature of the leaf pressing mold to rise to 110°C. After keeping warm for 10 minutes, remove the vegetation camouflage material from the mold after the water is dried and set aside.

[0058] Step 3: Add the molten material prepared in Step 1 to the non-woven fabric production line for melt extrusion, fiber forming, and wire drawing into a web in sequence, and then lay the vegetation camouflage material prepared in Step 2 on the upper surface of the semi-finished non-woven fabric web in a disordered manner. After the laying is completed, the vegetation camouflage material covers 30% of the upper surface of the non-woven fabric;

[0059] Step 4: Use the non-woven fabric spunlace process to reinforce the non-woven fabric semi-finished web and vegetation camouflage material in Step 3 by 2-3 times of needle punching process, and then put them into the non-woven fabric hot press for one-time hot pressing. The drum temperature of the non-woven fabric hot press is set to 127℃.

[0060] A camouflage absorbing non-woven fabric with a thickness of 0.8 mm was prepared and covered on the surface of the metal target to detect its absorption performance of electromagnetic waves. The radar electromagnetic waves in the frequency band of 1 to 40 GHz were used and the "bow method" was used for testing. The electromagnetic wave feedback attenuation data obtained are shown in Table 1:

[0061] Table 1

[0062]

[0063]

[0064] It can be seen that the non-woven fabric prepared by the formula of Example 1 has a good absorption rate for radar electromagnetic waves in the 1-40 GHz frequency band, especially in the 8-15 GHz frequency band, which can attenuate more than 90% of electromagnetic waves. The absorption rate of the vegetation camouflage material area for electromagnetic waves is slightly lower, forming a camouflage effect similar to leaves in radar imaging, and its radar imaging is as follows Figure 1 shown.

[0065] Embodiment 2 of the present invention:

[0066] Compared with Example 1, the components of 500 mesh iron powder and 50 nanometer nano silver powder are removed, and their weight parts are added to the nickel-iron alloy powder.

[0067] The weight parts of the formula raw materials are: 40.7 parts of polyacrylonitrile, 27.1 parts of polypropylene fiber, 11.05 parts of 500 mesh nickel-iron alloy powder, 3.15 parts of 500 mesh nickel powder, 3.48 parts of straw-based plant fiber, 8.72 parts of Lyocell fiber, 2.5 parts of methyl methacrylate and 2.1 parts of aluminate coupling agent.

[0068] The following steps are used to manufacture nonwoven fabrics:

[0069] Step 1: Preparation of chemical fiber base material: add parts by weight of polyacrylonitrile and polypropylene fiber granules into a high-temperature stirring tank, set the temperature to 240°C, stir for 5 minutes, and the stirring paddle speed is 90rpm. Then add parts by weight of nickel-iron alloy powder and nickel powder, set the temperature to 260°C, stir for 12 minutes to form a molten material for standby use, and the stirring paddle speed is 110rpm.

[0070] Step 2: Preparation of vegetation camouflage material: add 10 parts by weight of straw-based plant fiber particles into an extruder equipped with a leaf vein imitation mold, extrude at 175°C to form a plant leaf vein imitation shape, and then put it into a leaf pressing mold. Dissolve 10 parts by weight of Lyocell fiber particles in an aqueous solution with a pH value of 8.5 and a temperature of 75°C, and then add them through the gate of the leaf pressing mold. Control the temperature of the leaf pressing mold to rise to 110°C. After keeping warm for 10 minutes, remove the vegetation camouflage material from the mold after the water is dried and set aside.

[0071] Step 3: Add the molten material prepared in Step 1 to the non-woven fabric production line for melt extrusion, fiber forming, and wire drawing into a web in sequence, and then lay the vegetation camouflage material prepared in Step 2 on the upper surface of the semi-finished non-woven fabric web in a disordered manner. After the laying is completed, the vegetation camouflage material covers 30% of the upper surface of the non-woven fabric;

[0072] Step 4: Use the non-woven fabric spunlace process to reinforce the non-woven fabric semi-finished web and vegetation camouflage material in Step 3 by 2-3 times of needle punching process, and then put them into the non-woven fabric hot press for one-time hot pressing. The drum temperature of the non-woven fabric hot press is set to 127℃.

[0073] A camouflage absorbing non-woven fabric with a thickness of 0.8 mm was prepared and covered on the surface of the metal target to detect its absorption performance of electromagnetic waves. The radar electromagnetic waves in the frequency band of 1 to 40 GHz were used and the "bow method" was used for testing. The electromagnetic wave feedback attenuation data obtained are shown in Table 2:

[0074] Table 2

[0075]

[0076] It can be seen that the non-woven fabric prepared by the formula of Example 2 lacks the components of 500 mesh iron powder and 50 nanometer nano silver powder, and the absorption rate of radar electromagnetic waves in the frequency band of 1 to 40 GHz decreases significantly. After the overall absorption ratio of radar electromagnetic waves decreases, the overall absorption capacity of radar electromagnetic waves becomes weaker, which makes the non-woven fabric unsuitable for camouflage of military targets.

[0077] Embodiment 3 of the present invention:

[0078] Compared with Example 1, the components of straw-based plant fiber and Lyocell fiber are removed, and their weight parts are added to polyacrylonitrile and polypropylene fibers.

[0079] The weight parts of the formula raw materials are: 48 parts of polyacrylonitrile, 32 parts of polypropylene fiber, 11.05 parts of 500 mesh nickel-iron alloy powder, 3.15 parts of 500 mesh nickel powder, 3.48 parts of straw-based plant fiber, 8.72 parts of Lyocell fiber, 2.5 parts of methyl methacrylate and 2.1 parts of aluminate coupling agent.

[0080] The following steps are used to manufacture nonwoven fabrics:

[0081] Step 1: Preparation of chemical fiber base material: add parts by weight of polyacrylonitrile and polypropylene fiber granules into a high-temperature stirring tank, set the temperature to 240°C, stir for 5 minutes, and the stirring paddle speed is 90rpm. Then add parts by weight of nickel-iron alloy powder and nickel powder, set the temperature to 260°C, stir for 12 minutes to form a molten material for standby use, and the stirring paddle speed is 110rpm.

[0082] Step 2: Preparation of vegetation camouflage material: add 10 parts by weight of straw-based plant fiber particles into an extruder equipped with a leaf vein imitation mold, extrude at 175°C to form a plant leaf vein imitation shape, and then put it into a leaf pressing mold. Dissolve 10 parts by weight of Lyocell fiber particles in an aqueous solution with a pH value of 8.5 and a temperature of 75°C, and then add them through the gate of the leaf pressing mold. Control the temperature of the leaf pressing mold to rise to 110°C. After keeping warm for 10 minutes, remove the vegetation camouflage material from the mold after the water is dried and set aside.

[0083] Step 3: Add the molten material prepared in Step 1 to the non-woven fabric production line for melt extrusion, fiber forming, and wire drawing into a web in sequence, and then lay the vegetation camouflage material prepared in Step 2 on the upper surface of the semi-finished non-woven fabric web in a disordered manner. After the laying is completed, the vegetation camouflage material covers 30% of the upper surface of the non-woven fabric;

[0084] Step 4: Use the non-woven fabric spunlace process to reinforce the non-woven fabric semi-finished web and vegetation camouflage material in Step 3 by 2-3 times of needle punching process, and then put them into the non-woven fabric hot press for one-time hot pressing. The drum temperature of the non-woven fabric hot press is set to 127℃.

[0085] A camouflage absorbing non-woven fabric with a thickness of 0.8 mm was prepared and covered on the surface of the metal target to detect its absorption performance of electromagnetic waves. The radar electromagnetic waves in the frequency band of 1 to 40 GHz were used and the "bow method" was used for testing. The electromagnetic wave feedback attenuation data obtained are shown in Table 3:

[0086] Table 3

[0087]

[0088] It can be seen that after the non-woven fabric made by the formula of Example 3 lacks the component of vegetation camouflage material, the absorption rate of radar electromagnetic waves in the frequency band of 1 to 40 GHz remains basically unchanged, but such non-woven fabric has obvious block areas for radar imaging. Figure 2 Although the reconnaissance party does not know what is hidden in the area, it is easy to suspect that there are military targets in the area, which makes the non-woven fabric unsuitable as a camouflage for military targets.

[0089] The above are all preferred embodiments of the present invention, and are not intended to limit the protection scope of the present invention. Therefore, any equivalent changes made based on the structure, shape, and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A microwave-absorbing nonwoven fabric, characterized in that: The formula raw materials include the following components in parts by weight: 65-75 parts of chemical fiber base material, 10-15 parts of mixed metal powder for absorbing waves, 10-15 parts of vegetation camouflage material, 2-3 parts of methyl methacrylate and 2-3 parts of aluminate coupling agent; The chemical fiber base material is a mixture of polyacrylonitrile and polypropylene fibers, and the weight ratio of the polyacrylonitrile to the polypropylene fibers is 1.5:1; The mixed metal powder is composed of nickel-iron alloy powder, nickel powder, iron powder and nano silver powder, and the weight ratio of the nickel-iron alloy powder, nickel powder, iron powder and nano silver powder is 2:1:1:0.5; The particle sizes of the nickel-iron alloy powder, nickel powder and iron powder are all 500-1000 meshes, and the particle size of the nano silver powder is 10-100 nanometers; The vegetation camouflage material is made of straw-based plant fibers as simulated leaf veins, and Lyocell fibers are filled into the gaps of the straw-based plant fibers; The preparation method of the microwave-absorbing nonwoven fabric comprises the following specific steps: Step 1: Preparation of chemical fiber base material, add parts by weight of polyacrylonitrile and polypropylene fiber granules into a high-temperature stirring tank, set the temperature to 235-255°C, stir for 5 minutes, and rotate the stirring paddle at 90-95rpm, then add parts by weight of nickel-iron alloy powder, nickel powder, iron powder and nano silver powder, set the temperature to 255-265°C, stir for 10-15 minutes to form a molten material for standby use, and rotate the stirring paddle at 110-120rpm; Step 2: Preparation of vegetation camouflage material: add straw-based plant fiber particles into an extruder equipped with a leaf vein imitation mold, extrude at 150-200°C to form a leaf vein imitation shape, and then put it into a leaf pressing mold. Dissolve Lyocell fiber particles in an aqueous solution with a pH value of 8.0-8.7 and a temperature of 70-80°C, and then add them through the gate of the leaf pressing mold. Control the temperature of the leaf pressing mold to rise to 110°C, keep it warm for 10 minutes, and then demould and take out the vegetation camouflage material for use after the water is dried; Step 3: Add the molten material prepared in Step 1 to the non-woven fabric production line for melt extrusion, fiber forming, and wire drawing into a web in sequence, and then lay the vegetation camouflage material prepared in Step 2 on the upper surface of the semi-finished non-woven fabric web in a disordered manner. After the laying is completed, the vegetation camouflage material covers 60-75% of the upper surface of the non-woven fabric; Step 4: Use the non-woven spunlace process to reinforce the non-woven web semi-finished product and vegetation camouflage material in Step 3 through 2-3 times of needle punching process, and then enter the non-woven hot press for one-time hot pressing. The drum temperature of the non-woven hot press is set to 120-130℃.

2. The microwave-absorbing nonwoven fabric according to claim 1, characterized in that: The weight parts of the raw materials in the formula are: 68-71 parts of chemical fiber base material, 10-13 parts of mixed metal powder for absorbing waves, 10-13 parts of vegetation camouflage material, 2-3 parts of methyl methacrylate and 2-3 parts of aluminate coupling agent.

3. The microwave-absorbing nonwoven fabric according to claim 1, characterized in that: The weight parts of the formula raw materials are: 67.8 parts of chemical fiber base material, 14.2 parts of mixed metal powder for absorbing waves, 12.2 parts of vegetation camouflage material, 2.5 parts of methyl methacrylate and 2.1 parts of aluminate coupling agent.