Amorphous silicon thin film annealing method and device
By using the microwave annealing method in silicon-based heterogeneous cells, the problem of high defect density in amorphous silicon films is solved, the photoelectric conversion efficiency is improved, and the market demand for the performance of silicon-based heterogeneous cells is met.
Patent Information
- Application Number
- CN202310283197.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-22
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2043-03-22
AI Technical Summary
Amorphous silicon films are prone to defects during the production process, resulting in low photoelectric conversion efficiency of silicon-based heterojunction cells and inability to meet market demand.
An amorphous silicon film annealing method is adopted. By placing the parts to be processed in the process chamber, introducing protective gas and exhausting oxygen, microwave power is periodically loaded into the amorphous silicon film, and the total duration of the microwave power and each period are controlled. Power loading and stopping periods in the cycle to reduce the defect density of the amorphous silicon layer.
Through the microwave annealing method, the defect density of the amorphous silicon film is reduced, the photoelectric conversion efficiency is improved, the transformation of the crystal morphology is avoided, and the market demand for the performance of silicon-based heterogeneous cells is met.
Smart Images

Figure CN116314475B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of semiconductor manufacturing, and in particular to an amorphous silicon thin film annealing method and device. Background Art
[0002] At present, silicon-based heterogeneous batteries are becoming more and more popular in the market. In order to meet the needs of the market, silicon-based heterogeneous batteries have gradually entered the large-scale mass production stage.
[0003] However, due to various defects in the production process of amorphous silicon thin films, the photoelectric conversion efficiency of silicon-based heterojunction batteries may not be particularly high and cannot meet market demand. Summary of the invention
[0004] The present invention aims to solve at least one of the technical problems existing in the prior art, and proposes an amorphous silicon film annealing method and device to obtain an amorphous silicon film with a low defect density amorphous silicon layer.
[0005] In order to achieve the purpose of the present invention, a method for annealing an amorphous silicon film is provided, comprising: placing a workpiece to be processed on which the preparation of the amorphous silicon film is completed in a process chamber; introducing a protective gas into the process chamber and exhausting the gas in the process chamber at the same time until all the oxygen in the process chamber is exhausted; periodically loading microwave power to the amorphous silicon film to perform microwave annealing on the amorphous silicon film, and controlling the total duration of loading the microwave power as well as the power loading period and the power stopping period in each cycle to obtain an amorphous silicon film with a low defect density amorphous silicon layer.
[0006] Furthermore, the total duration of loading the microwave power is less than or equal to 5 seconds.
[0007] Further, the power loading period is less than or equal to 1 second.
[0008] Further, the power stop period is greater than or equal to 1 second and less than or equal to 2 seconds.
[0009] Furthermore, periodically loading microwave power onto the amorphous silicon film includes: detecting the temperature of the workpiece to be processed in real time, and issuing an over-temperature alarm when the temperature exceeds a set temperature and simultaneously stopping loading microwave power onto the amorphous silicon film.
[0010] Furthermore, the temperature was set to 140°C.
[0011] As another technical solution, the present invention also provides an amorphous silicon thin film annealing device, which is applied to the above-mentioned amorphous silicon thin film annealing method, and the annealing device includes: a process chamber, in which a carrying table for carrying a workpiece to be processed is arranged, and the process chamber is provided with an air inlet and an air outlet, the air inlet is used to introduce protective gas into the process chamber, and the air outlet is used to discharge the gas in the process chamber; a microwave source, which is arranged in the process chamber, and the microwave source is used to load microwave power to the amorphous silicon thin film; a control device, which is connected to the microwave source, and the control device is used to control the microwave source to periodically load microwave power to the amorphous silicon thin film.
[0012] Furthermore, the annealing device also includes: a detection device, which is arranged on the supporting platform, the detection device is used to detect the temperature of the workpiece to be processed and send the temperature to the control device; the control device is also used to issue an over-temperature alarm when the temperature exceeds the set temperature and simultaneously control the microwave source to stop loading microwave power.
[0013] Furthermore, the chamber wall of the process chamber is made of metal, or the inner surface of the chamber wall of the process chamber is provided with a metal layer, and the chamber wall made of metal or the inner surface of the metal layer is used to reflect microwaves irradiated thereon.
[0014] As another technical solution, the present invention further provides a processing device, including a processing device for preparing an amorphous silicon thin film and the above-mentioned amorphous silicon thin film annealing device.
[0015] As another technical solution, the present invention further provides a processing device, including the above-mentioned amorphous silicon thin film annealing device, wherein the process chamber in the amorphous silicon thin film annealing device is further integrated with a processing module for preparing the amorphous silicon thin film.
[0016] The present invention has the following beneficial effects:
[0017] The amorphous silicon thin film annealing method provided by the present invention comprises placing a workpiece to be processed after the preparation of the amorphous silicon thin film is completed in a process chamber; introducing a protective gas into the process chamber, and exhausting the gas in the process chamber at the same time until all the oxygen in the process chamber is exhausted; periodically loading microwave power to the amorphous silicon thin film to perform microwave annealing on the amorphous silicon thin film, and controlling the total duration of loading microwave power and the power loading period and power stop period in each cycle to obtain an amorphous silicon thin film with a low defect density amorphous silicon layer. Microwaves can cause the vibration of the silicon-hydrogen bond polarity bonds inside the amorphous silicon layer and the dangling bonds at the defects. Periodically loading microwaves can generate heat in a short time. Under the action of the heat, the defects of the amorphous silicon layer are passivated and repaired, and the defect density of the amorphous silicon layer in the amorphous silicon thin film part can be reduced. Periodically loading microwave power to the amorphous silicon thin film can also be understood as alternating between the power loading period and the power stop period, so as to intermittently load microwave power to the amorphous silicon thin film, so that the temperature of the amorphous silicon layer gradually increases. However, since the power loading period and power stopping period in each cycle are controlled, the microwave loading process is intermittently stopped to prevent the temperature of the amorphous silicon layer from rising too fast and crystallizing (crystal morphology transformation). The total duration of microwave power loading is also controlled, that is, the microwave power loading is stopped when the total duration of microwave power loading is reached, so that the temperature of the amorphous silicon film is increased to a level that can reduce the defect density of the amorphous silicon layer, but does not change the crystal morphology of the amorphous silicon layer.
[0018] The amorphous silicon thin film annealing device provided by the present invention includes a microwave source for loading microwave power onto the amorphous silicon thin film. Periodically loading microwave power onto the amorphous silicon thin film can also be understood as alternating power loading periods and power stopping periods, so as to intermittently load microwave power onto the amorphous silicon thin film, so that the temperature of the amorphous silicon layer gradually increases. However, since the power loading period and the power stopping period in each cycle are controlled, the loading of microwaves is intermittently stopped during the microwave loading process, so that the temperature of the amorphous silicon layer does not increase too quickly and crystallize (that is, the crystal morphology changes). The total duration of loading microwave power is also controlled, that is, the loading of microwave power is stopped when the total duration of loading microwave power is reached, so that the temperature of the amorphous silicon thin film is increased to a level that can reduce the defect density of its amorphous silicon layer, but does not change the crystal morphology of its amorphous silicon layer.
[0019] The processing equipment provided by the present invention includes a processing device for preparing an amorphous silicon film and an amorphous silicon film annealing device capable of obtaining an amorphous silicon film with an amorphous silicon layer having a low defect density. The amorphous silicon film annealing device can be used to perform microwave annealing on a workpiece to be processed after the preparation of the amorphous silicon film is completed, and the defects of the amorphous silicon layer of the amorphous silicon film can be passivated and repaired, so that an amorphous silicon film with an amorphous silicon layer having a low defect density can be obtained.
[0020] The processing equipment provided by the present invention includes an amorphous silicon film annealing device capable of obtaining an amorphous silicon film with a low defect density amorphous silicon layer. The process chamber in the amorphous silicon film annealing device is also integrated with a processing module for preparing the amorphous silicon film, and the amorphous silicon film can be prepared and annealed in the same process chamber.
[0021] Other objects and features of the present invention will become apparent by reading the specification, claims and drawings of the present application. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] The above and / or additional aspects and advantages of the present invention will become apparent and easily understood from the description of the embodiments in conjunction with the following drawings, in which:
[0023] Figure 1 4 is a flow chart of an amorphous silicon thin film annealing method according to an embodiment of the present invention.
[0024] Figure 2 It is a schematic structural diagram of an amorphous silicon thin film annealing device according to an embodiment of the present invention.
[0025] Description of main component symbols:
[0026] 10. Amorphous silicon thin film annealing device; 20. Parts to be processed;
[0027] 100, process chamber; 110, air inlet; 120, air outlet; 130, chamber wall; 140, outer wall of the chamber;
[0028] 200, bearing platform;
[0029] 300. Microwave source;
[0030] 400. Detection device;
[0031] 500. Control device;
[0032] 600. Power supply. DETAILED DESCRIPTION
[0033] The embodiments of the present invention are described in detail below, examples of which are shown in the accompanying drawings, wherein the same or similar reference numerals throughout represent the same or similar elements or elements having the same or similar functions. The embodiments described below with reference to the accompanying drawings are exemplary and are only used to explain the present invention, and cannot be understood as limiting the present invention.
[0034] In the description of the present invention, it should be understood that the orientation or positional relationship indicated by the terms "inside", "outside", etc. is based on the orientation or positional relationship shown in the accompanying drawings, and is only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation of the present invention. In addition, the terms "first" and "second" are only used for descriptive purposes, and cannot be understood as indicating or implying relative importance or implicitly indicating the number of technical features indicated. Therefore, the features defined as "first" and "second" may explicitly or implicitly include one or more of the features. In the description of the present invention, the meaning of "multiple" is two or more, unless otherwise clearly and specifically defined.
[0035] In the description of the present invention, it should be noted that, unless otherwise clearly specified and limited, the terms "installed", "connected", and "connected" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection, an electrical connection, or mutual communication; it can be a direct connection, or an indirect connection through an intermediate medium, it can be the internal connection of two elements or the interaction relationship between two elements. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.
[0036] The disclosure below provides many different embodiments or examples to realize different structures of the present invention. In order to simplify the disclosure of the present invention, the parts and settings of specific examples are described below. Of course, they are only examples, and the purpose is not to limit the present invention. In addition, the present invention can repeat reference numbers and / or reference letters in different examples, and this repetition is for the purpose of simplicity and clarity, which itself does not indicate the relationship between the various embodiments and / or settings discussed. In addition, the present invention provides various specific examples of processes and materials, but those of ordinary skill in the art can be aware of the application of other processes and / or the use of other materials.
[0037] In the description of this specification, the description with reference to the terms "one embodiment", "certain embodiments", "illustrative embodiments", "examples", "specific examples", or "some examples" means that the specific features, structures, materials, or characteristics described in conjunction with the embodiments or examples are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials, or characteristics described may be combined in any one or more embodiments or examples in a suitable manner.
[0038] Figure 1 FIG. 1 is a flow chart of an amorphous silicon thin film annealing method according to an embodiment of the present invention. Figure 1 , the amorphous silicon thin film annealing method includes:
[0039] S1001: placing the workpiece 20 on which the amorphous silicon thin film is prepared into the process chamber 100;
[0040] S1002: introducing a protective gas into the process chamber 100 and exhausting the gas in the process chamber 100 at the same time until all the oxygen in the process chamber 100 is exhausted;
[0041] S1003: Periodically load microwave power to the amorphous silicon film to perform microwave annealing on the amorphous silicon film, and control the total duration of loading microwave power as well as the power loading period and power stopping period in each cycle to obtain an amorphous silicon film with a low defect density amorphous silicon layer.
[0042] It should be noted that, when the amorphous silicon film is annealed in this embodiment, oxygen cannot exist in the process chamber 100 to avoid affecting it, and the amorphous silicon film needs to be placed in a protective gas atmosphere. After the process chamber 100 completes the step of exhausting oxygen, the process chamber 100 needs to be sealed. When microwave power is applied to the amorphous silicon film, the process chamber 100 needs to be in a sealed state to avoid microwave leakage and harm to the human body.
[0043] It can be understood that periodically loading microwave power to the amorphous silicon film means loading microwave power to the film at regular intervals, that is, loading power and stopping power loading are performed alternately and cyclically, and the duration of each cycle is a cycle. Specifically, each cycle includes a power loading period and a power stopping period. In other words, the power loading period and the power stopping period are performed alternately to intermittently load microwave power to the amorphous silicon film.
[0044] It should be noted that defect density is the number of defects per unit volume, where defects may include dangling bonds, interstitial atoms, etc.
[0045] The present invention anneals the amorphous silicon film by periodically loading microwaves (frequency greater than 300MHz) onto the amorphous silicon film. The microwaves can cause the silicon-hydrogen bond polarity bonds inside the amorphous silicon layer and the dangling bonds at the defects to vibrate without contacting the amorphous silicon film, thereby avoiding the contamination of the photovoltaic cell made of the amorphous silicon film. Moreover, when the microwaves are loaded onto the amorphous silicon film for annealing, both sides of the amorphous silicon film can be processed simultaneously without flipping the amorphous silicon film. Periodically loading microwaves can generate heat in a short time (annealing time is short, and the power consumption of the corresponding device will also be very low). Under the action of the heat, the defects of the amorphous silicon layer are passivated and repaired, and the defect density of the amorphous silicon layer in the amorphous silicon film component can be reduced. Periodically loading microwave power onto the amorphous silicon film can also be understood as alternating power loading periods and power stop periods, so that microwave power is intermittently loaded onto the amorphous silicon film, so that the temperature of the amorphous silicon layer gradually increases. However, since the power loading period and power stopping period in each cycle are controlled, the microwave loading will be stopped intermittently during the microwave loading process, so that the temperature of the amorphous silicon layer will not rise too quickly to crystallize (it can be understood that silicon is divided into crystalline and amorphous states according to the crystal form, and crystalline silicon is further divided into single crystal silicon and polycrystalline silicon. The amorphous state is amorphous silicon. Silicon materials in different forms have different structures. The crystal form transformation can be understood as the transformation of amorphous silicon into single crystal silicon or polycrystalline silicon or other forms of silicon layers). The total duration of microwave power loading is also controlled, that is, the microwave power loading is stopped when the total duration of microwave power loading is reached, so that the temperature of the amorphous silicon film is increased to a level that can reduce the defect density of its amorphous silicon layer, but will not change the crystal form of its amorphous silicon layer.
[0046] In some embodiments, the total duration of microwave power loading is less than or equal to 5 seconds. Since loading microwaves onto the amorphous silicon film will cause its temperature to rise, the temperature of the amorphous silicon film will also rise with the increase of the total duration of microwave power loading. In order to prevent the temperature of the amorphous silicon film from rising to the point where the amorphous silicon layer crystallizes (the amorphous silicon layer is transformed into polycrystalline silicon or other crystalline silicon), and considering that the portion of the amorphous silicon film where the amorphous silicon and crystalline silicon contact to form an interface is heated faster, the total duration of microwave power loading is limited to less than or equal to 5 seconds in this embodiment.
[0047] In some embodiments, the power loading period is less than or equal to 1 second. In order to prevent the amorphous silicon layer from being heated faster and crystallized due to a longer power loading period, the power loading period is limited to less than or equal to 1 second in this embodiment.
[0048] In some embodiments, the power stop period is greater than or equal to 1 second and less than or equal to 2 seconds. In order to avoid excessive temperature drop of the amorphous silicon film when the power is stopped, resulting in no or little reduction in the defect density of the amorphous silicon layer, the power stop period is limited to greater than or equal to 1 second and less than or equal to 2 seconds in this embodiment.
[0049] The following is explained with a specific example, but it can be understood that the present invention is not limited. Control the amorphous silicon film to load microwave power for 1 second, then stop for 1 second (no longer load microwave power to the amorphous silicon film), then load for 1 second, then stop for 1 second, then load for 1 second, then stop for 1 second, then load for 1 second, then stop for 1 second, then load for 1 second, then stop for 1 second, then load for 1 second, then stop for 1 second, then load for 1 second, at this time, the total duration of loading microwave power is 5 seconds, and the loading of microwave power is completely stopped, and annealing ends. In the above example, the power loading period and the power stopping period are alternated to intermittently load microwave power to the amorphous silicon film, so that the temperature of the amorphous silicon layer gradually increases, but because the microwave loading process will be stopped intermittently, the temperature of the amorphous silicon layer will not increase too fast and is not conducive to control. And the annealing is stopped when the total duration of loading microwave power is 5 seconds, so that the temperature of the amorphous silicon film is increased to reduce the defect density of its amorphous silicon layer, but will not change the crystal morphology of its amorphous silicon layer.
[0050] In some embodiments, periodically loading microwave power to the amorphous silicon film may include: real-time detection of the temperature of the amorphous silicon film, and when the temperature exceeds a set temperature, an over-temperature alarm is issued and simultaneously the loading of microwave power to the amorphous silicon film is stopped, so as to avoid the temperature of the amorphous silicon film being too high, causing the crystal morphology of the amorphous silicon layer to change (to polycrystalline silicon or other silicon layers).
[0051] The over-temperature alarm can be displayed on a display device, or a voice alarm, or a lamp with a color such as red can be used to remind the user. It is understandable that other methods that can be used to alarm can also be used.
[0052] Specifically, the set temperature is 140° C. Since the amorphous silicon film includes crystalline silicon and amorphous silicon, the portion where the amorphous silicon and the crystalline silicon contact to form an interface is heated faster. In order to prevent this portion of amorphous silicon from being converted into polycrystalline silicon or other crystalline silicon, the set temperature is set to 140° C., which is much lower than the temperature at which amorphous silicon is converted into polycrystalline silicon.
[0053] Figure 2 Schematic diagram of the structure of an amorphous silicon thin film according to an embodiment of the present invention. Figure 2The present invention also provides an amorphous silicon thin film annealing device 10, which is applied to the amorphous silicon thin film annealing method of the above embodiment. The amorphous silicon thin film annealing device 10 includes a process chamber 100, a microwave source 300 and a control device 500. A carrier 200 for carrying a workpiece 20 to be processed is provided in the process chamber 100, and the process chamber 100 is provided with an air inlet 110 and an air outlet 120. The air inlet 110 is used to introduce protective gas into the process chamber 100, and the air outlet 120 is used to discharge the gas in the process chamber 100. The microwave source 300 is provided in the process chamber 100, and the microwave source 300 is used to load microwave power to the amorphous silicon thin film. The control device 500 is connected to the microwave source 300, and the control device 500 is used to control the microwave source 300 to periodically load microwave power to the amorphous silicon thin film.
[0054] Specifically, the microwave source 300 is disposed on a side wall of the process chamber 100 .
[0055] The amorphous silicon thin film annealing device 10 further includes a detection device 400. The detection device 400 is disposed on the carrier 200, and is used to detect the temperature of the workpiece 20 to be processed, and send the temperature to the control device 500. The control device 500 is also used to issue an over-temperature alarm when the temperature exceeds the set temperature and simultaneously control the microwave source 300 to stop loading the microwave power.
[0056] In some embodiments, the detection device 400 may be disposed on a side of the carrier 200 close to the workpiece 20 to improve the accuracy of temperature detection.
[0057] In other embodiments, the carrying platform 200 itself may be provided with a detection device 400 , so that the carrying platform 200 can both carry the film of the workpiece 20 to be processed and detect the temperature of the workpiece 20 to be processed.
[0058] The chamber wall 130 of the process chamber 100 is made of metal, or the inner surface of the chamber wall 130 of the process chamber 100 is provided with a metal layer, and the chamber wall 130 made of metal or the inner surface of the metal layer is used to reflect the microwave irradiated thereon. And the inner surface of the chamber wall 130 made of metal or the metal layer can be a surface where microwaves are uniformly loaded to the amorphous silicon film.
[0059] In some embodiments, the process chamber 100 further includes an outer chamber wall 140 , and the outer chamber wall 140 is spaced apart from the chamber wall 130 .
[0060] In some embodiments, the present invention further provides a processing device, which includes a processing device for preparing an amorphous silicon thin film and an amorphous silicon thin film annealing device 10 of the above embodiment. In other words, the chamber of the processing device for preparing an amorphous silicon thin film and the process chamber 100 of the amorphous silicon thin film annealing device 10 are two different chambers, and the user needs to move the prepared amorphous silicon thin film from the processing device to the amorphous silicon annealing device before using the amorphous silicon annealing device to anneal the amorphous silicon thin film.
[0061] The following is an explanation using a specific example. First, place the sample coated with the amorphous silicon film together with the carrier on the carrier 200 to prevent the carrier 200 from rubbing against the sample and causing damage to it. Then seal the amorphous silicon annealing device. Subsequently, open the air inlet 110 and the air outlet 120, and pass an inert gas (for example, nitrogen or argon, etc.) into the process chamber 100 through the air inlet 110 as a protective gas. Since the inert gas enters the process chamber 100, the gas in the process chamber 100 will be discharged until all the oxygen in the process chamber 100 is discharged, and then close the air inlet 110 and the air outlet 120 at the same time to ensure that there is no interference from impurity gases. Finally, turn on the control device 500, the power supply 600 and the microwave source 300, and control the microwave source 300 through the control device 500 to periodically provide microwaves to the amorphous silicon film.
[0062] In other embodiments, the present invention further provides a processing device, which includes the amorphous silicon thin film annealing device 10 of the above embodiment, and the process chamber 100 in the amorphous silicon thin film annealing device 10 is also integrated with a processing module for preparing an amorphous silicon thin film. In other words, the chamber of the processing equipment for preparing an amorphous silicon thin film is the same chamber as the process chamber 100 of the amorphous silicon thin film annealing device 10, and the user does not need to remove the prepared amorphous silicon thin film from the process chamber 100, and can directly continue the annealing process in the process chamber 100.
[0063] It is understandable that the processing equipment may include a coating chamber (including a CVD chamber and a PVD chamber).
[0064] The following is an explanation of a specific example. First, the sample coated with the amorphous silicon film remains in the process chamber 100. Then the amorphous silicon annealing device is sealed (it is not necessary to introduce inert gas into the process chamber 100 at this time, but the glass observation window of the process chamber 100 needs to be replaced with glass coated with TCO to prevent microwave leakage and cause personal injury). Then the temperature of the sample is controlled to a certain range. Finally, the control device 500, the power supply 600 and the microwave source 300 are turned on, and the microwave source 300 is controlled by the control device 500 to periodically provide microwaves to the amorphous silicon film.
[0065] It is to be understood that the above embodiments are merely exemplary embodiments used to illustrate the principles of the present invention, but the present invention is not limited thereto. For those of ordinary skill in the art, various modifications and improvements can be made without departing from the spirit and essence of the present invention, and these modifications and improvements are also considered to be within the scope of protection of the present invention.
Claims
1. A method for annealing an amorphous silicon thin film, It is characterized in that include: Placing the workpiece to be processed after the preparation of the amorphous silicon thin film is completed in the process chamber; Introducing a protective gas into the process chamber and exhausting the gas in the process chamber at the same time until all the oxygen in the process chamber is exhausted; Periodically loading microwave power to the amorphous silicon film to perform microwave annealing on the amorphous silicon film, and controlling the total duration of loading the microwave power and the power loading period and the power stopping period in each cycle to obtain an amorphous silicon film having an amorphous silicon layer with a low defect density; Real-time detection of the temperature of the workpiece to be processed, and when the temperature exceeds a set temperature, an over-temperature alarm is issued and microwave power is stopped from being applied to the amorphous silicon film; The total time of loading the microwave power is less than or equal to 5 seconds; The power loading period is less than or equal to 1 second; The power stop period is greater than or equal to 1 second and less than or equal to 2 seconds; The set temperature is 140°C.
2. An amorphous silicon thin film annealing device, It is characterized in that The amorphous silicon thin film annealing method according to claim 1, wherein the annealing device comprises: A process chamber, wherein a carrying platform for carrying the workpiece to be processed is arranged therein, the process chamber is provided with an air inlet and an air outlet, the air inlet is used to introduce protective gas into the process chamber, and the air outlet is used to discharge the gas in the process chamber; A microwave source is disposed in the process cavity, and is used to apply microwave power to the amorphous silicon film; A control device connected to the microwave source, the control device being used to control the microwave source to periodically load microwave power to the amorphous silicon film; A detection device, disposed on the carrier platform, for detecting the temperature of the workpiece to be processed and sending the temperature to the control device; The control device is also used to issue an over-temperature alarm when the temperature exceeds a set temperature and simultaneously control the microwave source to stop loading microwave power.
3. The amorphous silicon thin film annealing device according to claim 2, It is characterized in that The chamber wall of the process chamber is made of metal, or the inner surface of the chamber wall of the process chamber is provided with a metal layer, and the chamber wall made of metal or the inner surface of the metal layer is used to reflect microwaves irradiated thereon.
4. A processing device, It is characterized in that The invention comprises a processing device for preparing an amorphous silicon thin film and an amorphous silicon thin film annealing device as claimed in claim 2 or 3.
5. A processing device, It is characterized in that It comprises the amorphous silicon thin film annealing device as claimed in claim 2 or 3, wherein the process chamber in the amorphous silicon thin film annealing device is also integrated with a processing module for preparing amorphous silicon thin film.