A modification method of a silicon oxide-supported nitrogen-containing carbon catalyst, supported carbon catalyst and application thereof

By modifying the nitrogen-containing carbon catalyst supported by silicon oxide, the problems of short catalyst life and high reaction temperature are solved, the activity and conversion rate of the catalyst are improved, the service life is extended, energy consumption is reduced, and coking phenomenon is reduced.

CN116328807BActive Publication Date: 2024-10-22DALIAN INSTITUTE OF CHEMICAL PHYSICS CHINESE ACADEMY OF SCIENCES +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111544009.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-12-16
Publication Date
2024-10-22
Estimated Expiration
2041-12-16

AI Technical Summary

Technical Problem

In the existing technology of cracking dichloroethane to produce vinyl chloride, the catalyst life is short and the reaction temperature is high, resulting in high energy consumption, low safety, and easy coking, requiring frequent coke removal and short production cycle.

Method used

The nitrogen-containing carbon catalyst supported by silicon oxide is used for modification. Through mixing, stirring, roasting and other steps with an alkaline solution, the silicon dioxide is removed, the specific surface area and pore volume of the catalyst are increased, and the skeleton structure of the catalyst is not destroyed, extending the service life.

Benefits of technology

The modified catalyst has an increased specific surface area, larger pore volume and pore diameter, higher conversion rate, longer catalyst service life, lowered reaction temperature, improved reaction selectivity, and reduced coking.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003415245550000061
    Figure BDA0003415245550000061
Patent Text Reader

Abstract

The present application discloses a modification method of a nitrogen-containing carbon catalyst supported by silicon oxide, a supported carbon catalyst and an application thereof, wherein the modification method comprises: mixing the nitrogen-containing carbon catalyst supported by silicon oxide with an alkaline solution, stirring, and drying to obtain a supported carbon catalyst. The method is a universal method, which is applicable to nitrogen-doped carbon-type catalysts supported by silicon oxide. The modification method of the catalyst adopts the technical scheme of alkaline leaching and desiliconization, and etches a part of the silicon oxide carrier of the catalyst supported by nitrogen-doped carbon, thereby increasing the specific surface area and pore volume of the catalyst, increasing the content of nitrogen-containing carbon active components of the catalyst, greatly improving the conversion rate of the catalyst, and prolonging the service life of the catalyst. The modification method is simple to operate and has low operating cost.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to a modification method of a silicon oxide-supported nitrogen-containing carbon catalyst, a supported carbon catalyst and an application thereof, and belongs to the field of catalysts. Background Art

[0002] Polyvinyl chloride (PVC for short) is a universal synthetic resin material widely used in the world. It is made by polymerizing the monomer vinyl chloride (VCM). There are two main methods for producing VCM. One is the acetylene hydrochloride addition route with mercuric chloride as the catalyst, and the other is the ethylene dichloride (EDC) cracking route with petroleum as the raw material. Due to the high potential toxicity of mercury and the serious mercury pollution of mercury catalysts, route 2 is gradually replacing route 1. It is of great significance to study the technology of preparing VCM by cracking ethylene dichloride. The technology of preparing vinyl chloride by cracking ethylene dichloride currently used in industry is thermal cracking technology without catalyst. The cracking temperature is 500-600℃, and the conversion rate of EDC is controlled at about 50%. Thermal cracking has a series of problems such as high reaction temperature, high energy consumption, low safety, easy coking, frequent coking, and short production cycle. The use of catalysts can greatly reduce the cracking reaction temperature, improve the reaction selectivity, and alleviate the coking degree of the reactor. Currently, most of the catalysts reported in patents are nitrogen-doped porous carbon catalysts (CN104289254B, CN105833892A, CN 104289247 A), which have the advantages of high EDC conversion rate and good product VCM selectivity. However, the carbon deposits and tar generated during the reaction will accumulate on the surface of the nitrogen-doped porous carbon material, resulting in a short catalyst life cycle. Summary of the invention

[0003] The present invention designs a supported carbon catalyst, which uses silicon dioxide as a carrier and the nitrogen-containing carbon loaded, which can keep the skeleton structure of the catalyst intact during ammonia regeneration and extend the service life of the catalyst. And because the carrier is a mesoporous structure, it is conducive to the diffusion of reactants and products. However, compared with ordinary activated carbon (800-2000m 2 / g), the specific surface area of ​​the silica carrier (200-400m 2 / g) is low, which is not conducive to improving the catalyst activity. Taking the above factors into consideration, in order to improve the performance (activity and life) of the EDC cracking catalyst, the EDC cracking catalyst should have a high specific surface area and a large pore size. A simple method to achieve these two requirements is to remove the silica on the supported carbon catalyst prepared in the early stage to increase the specific surface area and pore volume of the catalyst.

[0004] The supported carbon catalyst is treated with NaOH solution to remove silica. The chemical reaction principle is as follows:

[0005] SiO2+2NaOH→Na2SiO3+H2O.

[0006] In one aspect of the present application, a method for modifying a nitrogen-containing carbon catalyst supported on silicon oxide is provided, wherein the nitrogen-containing carbon catalyst supported on silicon oxide is mixed with an alkaline solution, stirred for reaction, separated, and calcined to obtain a supported carbon catalyst.

[0007] As a specific implementation, the modification method comprises:

[0008] Firstly, the nitrogen-containing carbon catalyst is immersed in an alkaline solution and heated and stirred, and then filtered and washed under reduced pressure, and finally dried at elevated temperature in an inert atmosphere to obtain a modified nitrogen-containing carbon catalyst.

[0009] Optionally, the alkaline solution is selected from one of NaOH, NaHCO3, Na2CO3, KOH, K2CO3, and KHCO3 solutions.

[0010] Optionally, in the alkaline solution, the mass fraction of alkali metal is 10% to 50%.

[0011] Optionally, the stirring conditions are: stirring temperature is 70-90° C.; heating rate is 0.1-20° C. / min; stirring time is 10-30 h.

[0012] Optionally, the calcination is carried out in an inactive atmosphere;

[0013] The inert atmosphere is selected from at least one of nitrogen or argon;

[0014] The calcination temperature is 100-200° C., and the drying time is 10-30 hours.

[0015] Optionally, the silicon oxide supported nitrogen-containing carbon catalyst comprises a catalyst having a nitrogen-doped carbon type;

[0016] The nitrogen element in the nitrogen-containing carbon is doped on the carbon material in the form of a covalent bond and is loaded on a silicon oxide carrier;

[0017] The mass content of the nitrogen element in the catalyst is 0.1-20%, the mass content of the carbon element in the catalyst is 20-99%, and the mass content of the silicon element in the catalyst is 0.1-80%.

[0018] Another aspect of the present application provides a supported carbon catalyst prepared by the above preparation method, wherein the supported carbon catalyst has a specific surface area of ​​1000 to 1800 m2 / g;

[0019] The pore volume of the supported carbon catalyst is 2 to 4 ml / g;

[0020] The pore size of the supported carbon catalyst is 2-7 nm.

[0021] The pore structure of the modified catalyst changed. The specific surface area increased from 200-400㎡ / g before modification to 1000-1800㎡ / g, the pore volume increased from 0.3-0.6ml / g to 2-4ml / g, and the pore diameter decreased from 10-20nm to 2-7nm. The pore diameter of the catalyst still maintained a mesoporous structure.

[0022] The weight loss of the modified catalyst is about 60-98%.

[0023] Another aspect of the present application provides a supported carbon catalyst prepared by the above preparation method or the use of the above supported carbon catalyst in catalyzing the dehydrohalogenation of halogenated hydrocarbons, the hydrochlorination of acetylene to prepare vinyl chloride, the preparation of vinyl chloride from acetylene and dichloroethane, the dehydrogenation of alkanes and ethylbenzene to prepare olefins, etc.

[0024] The beneficial effects of this application include:

[0025] (1) The modification method provided by the present invention has a wide range of applications, and is applicable to silicon oxide-supported nitrogen-doped or non-doped carbon materials with other atoms, wherein nitrogen-containing carbon is used as an active component, and the modification using the method is beneficially improved.

[0026] (2) The pore structure of the modified catalyst is improved, the specific surface area is increased, the pore volume is increased, and the most probable pore diameter is enlarged.

[0027] (3) The nitrogen-carbon loading of the modified catalyst is significantly increased, and the catalyst conversion rate is greatly improved.

[0028] (4) The modified catalyst has a greatly increased pore volume, so that the carbon produced during some reactions that are prone to carbon deposition can be accommodated in the pores, thereby extending the service life of the catalyst. DETAILED DESCRIPTION

[0029] The present application is described in detail below with reference to embodiments, but the present application is not limited to these embodiments.

[0030] Unless otherwise specified, the raw materials and catalysts in the examples of the present application were purchased through commercial channels, wherein the silica gel beads were purchased from Shandong Dongying Yiming New Materials Co., Ltd., 80 to 120 mesh coarse pore microsphere silica gel, white in color.

[0031] The analysis method in the examples of this application is as follows:

[0032] The nitrogen content was determined by an EA3000 elemental analyzer from Lehmann.

[0033] The specific surface area, pore volume and pore distribution were measured by a physical adsorption instrument from Quantachrome.

[0034] The conversion rate of 1,2-dichloroethane and the selectivity of vinyl chloride were determined by fixed bed reactor analysis. 1,2-dichloroethane was bubbled into the reactor under nitrogen. The nitrogen flow rate was 2.5 ml / min, the bubbling temperature was 5°C, the catalyst loading was 0.2 g, and the bed residence time was 18.1 s.

[0035] In the present application, the modified catalyst is used for the cracking of 1,2-dichloroethane to produce vinyl chloride. The reaction has an induction period, during which the conversion rate gradually increases with the extension of the reaction time and stabilizes after 3 days.

[0036] In the examples of this application, the conversion rate and selectivity are calculated as follows:

[0037] In the examples of the present application, the conversion rate of 1,2-dichloroethane and the selectivity of vinyl chloride are calculated based on the number of moles:

[0038] Conversion rate of 1,2-dichloroethane = 1,2-dichloroethane consumed in the reaction (mol) / 1,2-dichloroethane passed into the reactor (mol)

[0039] Vinyl chloride selectivity = vinyl chloride produced by the reaction (mol) / total of all products produced by the reaction (mol)

[0040] Example 1

[0041] In a 3L beaker, add 500.05g of deionized water ice cubes, 1.70L of deionized water, add 501.20g of sodium hydroxide, add the supported carbon catalyst Fresh-Cat# in Comparative Example 1 after dissolving, heat to 80.0°C in a water bath, stir mechanically for 24 hours to remove silica, filter in a Buchner funnel, and wash with 5.0L of deionized water (add about 1.0L of deionized water each time).

[0042] The washed carbon catalyst was placed in a rotary tube furnace with a nitrogen flow rate of 500 mL / min, and the temperature was increased to 120.0°C at 2°C / min, and dried at the constant temperature for 12 hours.

[0043] The sample weight of the supported carbon catalyst before modification was 478.52 g, and the sample weight after removal of silica was 121.13 g.

[0044] Example 2

[0045] The difference from Example 1 is that the amount of NaOH added is 250 g.

[0046] Example 3

[0047] The difference from Example 1 is that the stirring temperature is 90°C.

[0048] Example 4

[0049] The difference from Example 1 is that the stirring time is 10 h.

[0050] Example 5

[0051] The difference from Example 1 is that the added alkaline solution is KOH alkaline solution.

[0052] The catalysts of Examples 1-5 were subjected to the same evaluation process as the comparative example, reacted at 250°C, and after stabilization during the induction period, the selectivity of vinyl chloride was 99%, and the conversion rate of 1,2-dichloroethane was above 50%.

[0053] Comparative Example 1

[0054] Add 200 mL of furan methanol into a 1000 mL beaker at room temperature, add 2.00 g of oxalic acid while stirring, add 300 mL of xylene after dissolution, add 500 mL of coarse-pore microsphere silica gel into the beaker and place it in a 20°C water bath, soak for 6 hours, filter to remove excess liquid, put it into a 1000 mL beaker, polymerize in a 60°C water bath for 12 hours, heat to 90°C and polymerize for another 12 hours.

[0055] Take 500 mL of coarse-porous silica gel balls soaked in furan methanol, put them into a quartz tube of a rotary tube furnace, and introduce nitrogen at a flow rate of 250 mL / min for 4 hours to replace the air and dry the soaked balls. In the rotary tube furnace, heat up to 150°C at 1°C / min under nitrogen protection, keep the temperature constant for 3 hours, then heat up to 450°C at 1°C / min, keep the temperature constant for 3 hours, and then cool to room temperature.

[0056] After cooling under nitrogen, the nitrogen flow rate was changed to 45mL / min, the ammonia flow rate was 180mL / min, the temperature was kept constant for 2 hours before heating to replace the gas, the temperature was raised to 800℃ at 5℃ / min, the temperature was kept constant for 1.5 hours, the ammonia was stopped, the nitrogen flow rate was changed to 250mL / min, the temperature was lowered to 600℃ at 5℃ / min, the temperature was kept constant for 1.5 hours, and it naturally dropped to room temperature. The mass percentage of nitrogen in the loaded nitrogen-containing carbon material is 4.1%. It is recorded as Fresh-Cat#.

[0057] 1,2-dichloroethane was bubbled into a fixed bed reactor loaded with a catalyst, the reactor temperature was 250°C, and the residence time of 1,2-dichloroethane was (GHSV) 18.1s. The test results showed that the conversion rate of 1,2-dichloroethane was 18.5% and the selectivity of vinyl chloride was 99%.

[0058]

[0059] The above are only a few embodiments of the present application and do not constitute any form of limitation to the present application. Although the present application is disclosed as above with preferred embodiments, it is not intended to limit the present application. Any technician familiar with the profession, without departing from the scope of the technical solution of the present application, using the technical content disclosed above to make slight changes or modifications are equivalent to equivalent implementation cases and fall within the scope of the technical solution.

Claims

1. An application of a supported carbon catalyst in the reaction of preparing vinyl chloride from ethylene dichloride, characterized in that: The nitrogen-containing carbon catalyst supported by silicon oxide is mixed with an alkaline solution, stirred for reaction, separated, and calcined to obtain a supported carbon catalyst; The specific surface area of ​​the supported carbon catalyst is 1000-1800m 2 / g; The pore volume of the supported carbon catalyst is 2-4 ml / g; The pore size of the supported carbon catalyst is 2-7 nm; The alkaline solution is selected from one of NaOH, NaHCO3, Na2CO3, KOH, K2CO3, and KHCO3 solutions; The silicon oxide supported nitrogen-containing carbon catalyst includes a catalyst having a nitrogen-doped carbon type; The nitrogen element in the nitrogen-containing carbon is doped on the carbon material in the form of a covalent bond and is loaded on a silicon oxide carrier; The mass content of the nitrogen element in the catalyst is 0.1-20%, the mass content of the carbon element in the catalyst is 20-99%, and the mass content of the silicon element in the catalyst is 0.1-80%; The pore size of the supported carbon catalyst still maintains the mesoporous structure.

2. The use according to claim 1, characterized in that: In the alkaline solution, the mass fraction of the alkali metal is 10% to 50%.

3. The use according to claim 1, characterized in that: The stirring conditions are: stirring temperature is 70-90° C.; stirring time is 10-30 h.