Preparation method of Zn-Fe-N / C persulfate activator derived from bimetallic ZIF, its products and applications

Through high-temperature pyrolysis treatment of ZIF (Zn, Fe) bimetal-based materials, Zn-Fe-N/C persulfate activator is prepared, which solves the problems of poor catalyst cycle stability and metal dissolution, and achieves efficient organic pollution in water. It removes substances, reduces the risk of secondary pollution of water quality, and is suitable for sewage treatment.

CN116328809BActive Publication Date: 2024-10-22NAT NANOTECHNOLOGY STAR(SHANGHAI) DEV CO LTD +1

Patent Information

Application Number
CN202211695441.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-28
Publication Date
2024-10-22
Estimated Expiration
2042-12-28

AI Technical Summary

Technical Problem

Existing MOF catalysts have poor cycle stability and metal-organic framework collapse problems during the catalytic process, resulting in secondary pollution of water quality. Traditional advanced oxidation technology has limitations such as secondary pollution of metal ions and high energy consumption.

Method used

ZIF (Zn, Fe) bimetal-based material is used as the precursor, and through high-temperature pyrolysis treatment, the Zn/Fe ratio and pyrolysis temperature are controlled, the Zn-Fe-N/C persulfate activator is synthesized, and the active components are controlled. content and product size structure, reduce metal dissolution rate, and improve catalytic stability and efficiency.

Benefits of technology

It effectively reduces the metal dissolution rate, enhances the structural stability and catalytic activity of the material, improves the removal efficiency of organic pollutants in water, maintains the high efficiency stability and catalytic activity of the catalyst, and is suitable for sewage treatment.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present invention relates to a preparation method of a Zn-Fe-N / C persulfate activator derived from a bimetallic ZIF, and its products and applications, that is, a method of high-temperature pyrolysis of a bimetallic ZIF material is used to obtain a derived Zn-Fe-N / C material with a dodecahedral metal-organic framework structure, and the morphology structure and surface active component content of the derived material can be reasonably controlled by regulating the Zn and Fe molar ratios and the pyrolysis temperature and time, and the synergistic effect between metals can also avoid the metal dissolution problem in the degradation process of persulfate activated oxidative pollutants. In addition, the catalyst has good magnetic properties, can effectively solve the problem of catalyst recovery, and exhibits excellent catalytic stability, providing a new perspective for the design and application of heterogeneous bimetallic persulfate activators.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a preparation method of a bimetallic ZIF-derived Zn-Fe-N / C persulfate activator, a product thereof and an application thereof, which can effectively regulate the structure of the material and its catalytic stability, improve the recycling of the catalyst and be used in the field of sewage treatment. Background Art

[0002] Water pollution is still a difficult problem that we are facing. Although traditional technologies have alleviated and covered up its adverse effects on human health and environmental ecosystems to a certain extent, the treatment efficiency is not significant and secondary pollution is prone to occur, which still needs further research. Among various technologies, advanced oxidation process is a treatment method that can efficiently remove organic compounds from aquatic media. Common advanced oxidation technology is mainly based on H2O2 to generate active hydroxyl radicals ·OH for mineralization of organic matter. Compared with ·OH, SO4 - ·It has stronger oxidation ability, longer life and higher selectivity. Therefore, in recent years, SO4 - · Advanced oxidation technologies, which are mainly based on SO4 -· It can be activated by different methods, such as heat, light, electricity, ultrasound, catalyst, etc. Among these activation methods, transition metal activation is the most preferred, which not only has high activation efficiency, but also does not require additional energy, has low energy consumption and low processing cost. However, homogeneous catalysis is easily limited by secondary pollution of metal ions and high catalyst consumption. In persulfate activation, iron-based heterogeneous catalysts stand out because of their low cost and high efficiency. In particular, heterogeneous metal catalysts derived from metal organic framework materials, a multifunctional hybrid material, have attracted widespread attention due to their porous structure and well-dispersed active sites. Among various MOFs, zeolite imidazolate framework (ZIF) has the characteristics of large specific surface area, high porosity, a large number of dispersed metal ions, and good chemical and thermal stability. ZIF-8 is one of the typical ZIF materials and has been widely used in catalytic degradation of organic pollutants in water. However, heterogeneous catalysts derived from ZIF-8 still face the problem of secondary water pollution caused by metal dissolution, which is also a technical bottleneck in practical applications. Studies have found that Zn in ZIF-8 can be used as a carrier to disperse Fe ions, so that iron ions can be successfully further converted into corresponding ZIFs, and then a bimetallic metal-organic framework material is synthesized, which is beneficial to enhance charge transfer and improve catalytic activity. Therefore, the present patent application uses the synthesized ZIF (Zn, Fe) bimetallic MOF material as a precursor, and synthesizes Zn-Fe-N / C with different Zn contents through high-temperature pyrolysis. Through the synergistic effect between different metals, the metal dissolution rate is effectively reduced and the structural stability of the material is enhanced. Moreover, this method can control the content of active components and the size structure of the product by effectively adjusting the ratio of reaction raw materials, reaction temperature and time, thereby improving its removal efficiency of organic pollutants in water. After multiple cycles, the pollutants can still be well removed, and the catalyst maintains efficient stability and catalytic activity. Summary of the invention

[0003] In view of the problems of poor cyclic stability and metal-organic framework collapse of current MOF catalysts during catalysis, the present invention aims to provide a method for preparing a bimetallic ZIF-derived Zn-Fe-N / C persulfate activator.

[0004] Another object of the present invention is to provide a Zn-Fe-N / C persulfate activator product derived from a bimetallic ZIF prepared by the above method.

[0005] Another object of the present invention is to provide an application of the above product.

[0006] The object of the present invention is achieved by the following scheme: A method for preparing a Zn-Fe-N / C persulfate activator derived from a Zn-Fe bimetallic ZIF, characterized in that a ZIF precursor is subjected to high-temperature pyrolysis treatment, and the size and residual Zn content of the derivative product can be effectively adjusted by regulating the Zn / Fe ratio and the pyrolysis temperature, thereby improving the persulfate activation ability, and specifically comprising the following steps:

[0007] (1) Under magnetic stirring, Zn(NO3)3·6H2O and Fe(NO3)3·9H2O were placed in methanol solvent according to a certain Zn / Fe molar ratio and mixed evenly;

[0008] (2) Weigh a certain amount of 2-methylimidazole and dissolve it in methanol solvent;

[0009] (3) Add the solution in (1) dropwise into (2) while controlling the dropping rate; after the dropping is complete, subject the mixture to ultrasonic cavitation at room temperature for a period of time and then stir for 1 hour to obtain the ZIF (Zn, Fe) precursor;

[0010] (4) centrifugally washing the product in (3), freeze-drying it, and controlling the freeze-drying time;

[0011] (5) After drying, place it in a tube furnace for high-temperature pyrolysis, and control the calcination atmosphere, calcination temperature and calcination time;

[0012] (6) The product of (5) is subjected to a secondary low-temperature oxidation treatment, and the heating temperature and time are controlled to obtain a ZIF-derived Zn-Fe-N / C persulfate activator.

[0013] The Zn:Fe molar ratio is (5-20):1;

[0014] The drop acceleration rate is 1-2s / drop, and the ultrasonic time is 30min;

[0015] The freeze drying time is 12 to 24 hours;

[0016] The tube furnace calcination atmosphere is nitrogen or H2 / Ar mixed gas, and the calcination temperature and calcination time are 700-900°C and 2-6h respectively;

[0017] The secondary oxidation treatment temperature and time are 25-60° C. and 2-10 hours respectively.

[0018] The invention provides a Zn-Fe-N / C persulfate activator derived from a Zn-Fe bimetallic ZIF, which is prepared according to any one of the above methods.

[0019] The invention provides an application of a Zn-Fe-N / C persulfate activator derived from a Zn-Fe bimetallic ZIF in treating a RhB solution.

[0020] The catalytic experiment of ZIF-derived Zn-Fe-N / C persulfate activator was carried out in a beaker. A certain amount of Zn-Fe-N / C was added to 50 ml of 50 mg / L RhB solution. After stirring for 60 minutes to reach adsorption-desorption equilibrium, potassium persulfate was added to the solution for catalytic degradation for 30 minutes. Samples were taken and filtered with a filter to determine the mineralization rate of RhB.

[0021] A bimetallic ZIF metal-organic framework material is used as a precursor. The synergistic effect between metals is utilized to improve the stability of the material while also facilitating the improvement of the electron transmission capacity. At the same time, the size of the material and the content of the surface active components are controlled by controlling the raw material ratio and the synthesis temperature, thereby obtaining a method for preparing a controllable heterogeneous catalyst.

[0022] The present invention has the following advantages:

[0023] (1) The present invention proposes a method for preparing a Zn-Fe-N / C persulfate activator derived from a Zn-Fe bimetallic ZIF and its application. The Zn-Fe-N / C activator derived from a Zn-Fe bimetallic ZIF material is used as a precursor. The Zn-Fe-N / C activator obtained by high-temperature pyrolysis not only retains its dodecahedral skeleton structure well, but also the C layer plays an important role in stabilizing the structure and improving the activity, thereby promoting the transmission of electrons and accelerating the generation of sulfate radicals.

[0024] (2) The Zn-Fe-N / C persulfate activator proposed in the present invention can change the Zn residual ratio and the size structure of the catalyst by adjusting the Zn / Fe molar ratio and the high-temperature reaction temperature and time, thereby adjusting the content of the active component and accelerating the electron transfer and surface catalytic reaction rate.

[0025] (3) The preparation method of the bimetallic Zn-Fe-N / C persulfate activator proposed in the present invention is not only simple and controllable, but also has a rich pore structure and good stability. The activation rate of active free radicals is fast, thereby accelerating the oxidative degradation of pollutants in water, and has broad application prospects. DETAILED DESCRIPTION

[0026] The present invention is further described by way of examples.

[0027] Embodiment 1:

[0028] A Zn-Fe-N / C persulfate activator derived from a Zn-Fe bimetallic ZIF is prepared by high-temperature pyrolysis of a ZIF precursor, and the size and residual Zn content of the derived product can be effectively adjusted by regulating the Zn / Fe ratio and the pyrolysis temperature, thereby improving the ability to activate persulfate. The activator is prepared according to the following steps:

[0029] (1) Under magnetic stirring, Zn(NO3)3·6H2O and Fe(NO3)3·9H2O were placed in methanol solvent at a Zn:Fe molar ratio of 20:1 and mixed evenly;

[0030] (2) Dissolve 2-methylimidazole in methanol solvent, and add a slight excess of 2-methylimidazole to prepare a supersaturated solution;

[0031] (3) Add the solution in (1) dropwise into (2) at a rate of 2 s / drop; after the addition is complete, perform ultrasonic cavitation at room temperature for 30 min, and then stir for 1 h to obtain the ZIF (Zn, Fe) precursor;

[0032] (4) The ZIF (Zn, Fe) precursor product in (3) was centrifuged and washed, and then freeze-dried, and the freeze-drying time was controlled to 24 h;

[0033] (5) After drying, place it in a tube furnace for high-temperature pyrolysis, control the calcination atmosphere to be a H2 / Ar mixed gas, and calcine at 800°C for 2h;

[0034] (6) The product of (5) was subjected to a secondary low-temperature oxidation treatment, with the heating temperature controlled at 25 °C and the heating time controlled at 2 h, to obtain a ZIF-derived Zn-Fe-N / C persulfate activator.

[0035] The mineralization rate of the prepared catalyst to RhB solution was 75.9%.

[0036] Embodiment 2:

[0037] A Zn-Fe-N / C persulfate activator derived from a Zn-Fe bimetallic ZIF was prepared by the following steps similar to those in Example 1:

[0038] (1) Under magnetic stirring, Zn(NO3)3·6H2O and Fe(NO3)3·9H2O were placed in methanol solvent at a Zn / Fe molar ratio of 20:1 and mixed evenly;

[0039] (2) Dissolve 2-methylimidazole in methanol solvent;

[0040] (3) Add the solution in (1) dropwise into (2) at a rate of 1 s / drop; after the addition is complete, perform ultrasonic cavitation at room temperature for 30 min, and then stir for 1 h to obtain the ZIF (Zn, Fe) precursor;

[0041] (4) The product in (3) is centrifuged and washed, and then freeze-dried, and the freeze-drying time is controlled to be 24 hours;

[0042] (5) After drying, the product was placed in a tubular furnace for high-temperature pyrolysis, and the calcination atmosphere was controlled to be a H2 / Ar mixed gas. The calcination temperature and calcination time were 900°C and 6h, respectively;

[0043] (6) The product of (5) is subjected to a secondary low-temperature oxidation treatment, and the heating temperature and time are controlled to be 40°C and 2 h to obtain a ZIF-derived Zn-Fe-N / C persulfate activator.

[0044] The mineralization rate of the prepared catalyst to RhB solution was 67.5%.

[0045] Embodiment 3:

[0046] A Zn-Fe-N / C persulfate activator derived from a Zn-Fe bimetallic ZIF was prepared by the following steps similar to those in Example 1:

[0047] (1) Under magnetic stirring, Zn(NO3)3·6H2O and Fe(NO3)3·9H2O were placed in methanol solvent at a Zn / Fe molar ratio of 10:1 and mixed evenly;

[0048] (2) Dissolve 2-methylimidazole in methanol solvent;

[0049] (3) Add the solution in (1) dropwise into (2) at a rate of 1 s / drop; after the addition is complete, perform ultrasonic cavitation at room temperature for 30 min, and then stir for 1 h to obtain the ZIF (Zn, Fe) precursor;

[0050] (4) The product in (3) is centrifuged and washed, and then freeze-dried, and the freeze-drying time is controlled to be 24 hours;

[0051] (5) After drying, place it in a tubular furnace for high-temperature pyrolysis, control the calcination atmosphere to be a nitrogen mixed gas, and the calcination temperature and calcination time are 800°C and 4h respectively;

[0052] (6) The product of (5) is subjected to a secondary low-temperature oxidation treatment, and the heating temperature and time are controlled to be 25°C and 2 h to obtain a ZIF-derived Zn-Fe-N / C persulfate activator.

[0053] The mineralization rate of the prepared catalyst to RhB solution was 51.3%.

[0054] Embodiment 4:

[0055] A Zn-Fe-N / C persulfate activator derived from a Zn-Fe bimetallic ZIF was prepared by the following steps similar to those in Example 1:

[0056] (1) Under magnetic stirring, Zn(NO3)3·6H2O and Fe(NO3)3·9H2O were placed in methanol solvent at a Zn / Fe molar ratio of 10:1 and mixed evenly;

[0057] (2) Dissolve 2-methylimidazole in methanol solvent;

[0058] (3) Add the solution in (1) dropwise into (2) at a rate of 2 s / drop; after the addition is complete, perform ultrasonic cavitation at room temperature for 30 min, and then stir for 1 h to obtain the ZIF (Zn, Fe) precursor;

[0059] (4) The product in (3) was centrifuged and washed, and then freeze-dried, and the freeze-drying time was controlled to be 12 h;

[0060] (5) After drying, the product was placed in a tube furnace for high-temperature pyrolysis, and the calcination atmosphere was controlled to be a H2 / Ar mixed gas. The calcination temperature and calcination time were 800°C and 6h, respectively;

[0061] (6) The product of (5) is subjected to a secondary low-temperature oxidation treatment, and the heating temperature and time are controlled to be 25°C and 10 h, thereby obtaining a ZIF-derived Zn-Fe-N / C persulfate activator.

[0062] The mineralization rate of the prepared catalyst to RhB solution was 71.4%.

Claims

1. A method for preparing a bimetallic ZIF-derived Zn-Fe-N / C persulfate activator, characterized in that: The ZIF precursor is subjected to high temperature pyrolysis treatment, and the Zn / Fe ratio and the pyrolysis temperature are regulated to effectively adjust the size of the derivative product and the residual Zn content, thereby improving the persulfate activation ability, comprising the following steps: (1) Under magnetic stirring, Zn(NO3)3·6H2O and Fe(NO3)3·9H2O were placed in methanol solvent at a Zn:Fe molar ratio of (5-20):1 and mixed evenly; (2) Dissolve 2-methylimidazole in methanol solvent; (3) Add the solution in (1) dropwise into (2). After the addition is complete, subject the mixture to ultrasonic cavitation at room temperature for a period of time and then stir for 1 h to obtain the ZIF (Zn, Fe) precursor. (4) centrifugally washing the ZIF (Zn, Fe) precursor product in (3), and then freeze-drying the product and controlling the freeze-drying time; (5) After drying, place it in a tube furnace for high-temperature pyrolysis, and control the calcination atmosphere, calcination temperature and calcination time; (6) subjecting the product of (5) to secondary low-temperature oxidation treatment, controlling the heating temperature and time, to obtain a ZIF-derived Zn-Fe-N / C persulfate activator; In step (3), the drop acceleration rate is 1-2 s / drop, and the ultrasonic time is 30 min; In step (4), the freeze-drying time is 12 to 24 hours; In step (5), the tubular furnace calcination atmosphere is nitrogen or H2 / Ar mixed gas, and the calcination temperature and calcination time are 700-800°C and 2-6h, respectively.

2. The method for preparing a bimetallic ZIF-derived Zn-Fe-N / C persulfate activator according to claim 1, characterized in that: In step (6), the temperature and time of the secondary low-temperature oxidation treatment are 25-60° C. and 2-10 h, respectively.

3. A method for preparing a bimetallic ZIF-derived Zn-Fe-N / C persulfate activator according to any one of claims 1 to 2, characterized in that: Prepare as follows: (1) Under magnetic stirring, Zn(NO3)3·6H2O and Fe(NO3)3·9H2O were placed in methanol solvent at a Zn:Fe molar ratio of 20:1 and mixed evenly; (2) Dissolve 2-methylimidazole in methanol solvent; (3) Add the solution in (1) dropwise into (2) at a rate of 2 s / drop; after the addition is complete, perform ultrasonic cavitation at room temperature for 30 min, and then stir for 1 h to obtain the ZIF (Zn, Fe) precursor; (4) The ZIF (Zn, Fe) precursor product in (3) was centrifuged and washed, and then freeze-dried, and the freeze-drying time was controlled to 24 h; (5) After drying, place it in a tube furnace for high-temperature pyrolysis, control the calcination atmosphere to be a H2 / Ar mixed gas, and calcine at 800°C for 2h; (6) The product of (5) was subjected to a secondary low-temperature oxidation treatment, with the heating temperature controlled at 25 °C and the heating time controlled at 2 h, to obtain a ZIF-derived Zn-Fe-N / C persulfate activator.

4. A method for preparing a bimetallic ZIF-derived Zn-Fe-N / C persulfate activator according to any one of claims 1 to 2, characterized in that: Prepare as follows: (1) Under magnetic stirring, Zn(NO3)3·6H2O and Fe(NO3)3·9H2O were placed in methanol solvent at a Zn / Fe molar ratio of 10:1 and mixed evenly; (2) Dissolve 2-methylimidazole in methanol solvent; (3) Add the solution in (1) dropwise into (2) at a rate of 2 s / drop; after the addition is complete, ultrasonic cavitation is performed at room temperature for 30 min, followed by stirring for 1 h to obtain a ZIF (Zn, Fe) precursor; (4) The product in (3) was centrifuged and washed, and then freeze-dried, and the freeze-drying time was controlled to be 12 h; (5) After drying, the product was placed in a tubular furnace for high-temperature pyrolysis, and the calcination atmosphere was controlled to be a H2 / Ar mixed gas. The calcination temperature and calcination time were 800°C and 6h, respectively; (6) subjecting the product of (5) to a secondary low-temperature oxidation treatment, controlling the heating temperature and time to 25°C and 10 h, to obtain a ZIF-derived Zn-Fe-N / C persulfate activator; The mineralization rate of the prepared persulfate activator for RhB solution was 71.4%.

5. A bimetallic ZIF-derived Zn-Fe-N / C persulfate activator, characterized in that Prepared according to any one of claims 1 to 4.

6. Use of the Zn-Fe-N / C persulfate activator derived from the bimetallic ZIF according to claim 5 in treating RhB solution.

Citation Information

Patent Citations

  • Carbon-containing iron-based catalyst for hydrogenation of CO2 to prepare hydrocarbons, and preparation method thereof

    CN110404575A

  • ZIF-8-derived hollow Fe / Cu-N-C type oxygen reduction catalyst and preparation method and application thereof

    CN110752380A

  • Aza porous carbon loaded transition metal NPs / SAs double-active-site electrocatalyst as well as preparation method and application of aza porous carbon loaded transition metal NPs / SAs double-active-site electrocatalyst

    CN113755889A

  • Preparation method of catalyst with metal organic framework structure as well as product and application of catalyst

    CN114011410A

  • MOFs-derived Fe-N / C catalyst containing defect Fe-Nx as well as preparation method and application of MOFs-derived Fe-N / C catalyst

    CN115041211A

Cited By

  • Efficient preparation method of ZnFe-ZIF material at normal temperature and pressure

    CN122213435A