A carrier-modified catalyst and its preparation method and application

By modifying the carrier of the VOCs exhaust gas catalyst and encapsulating precious metal single atoms, the problems of carrier micro-roughness and high precious metal loading rate are solved, the performance and life of the catalyst are improved, and efficient purification effects are achieved under complex working conditions.

CN116328818BActive Publication Date: 2024-10-25ZHEJIANG UNIV +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310229430.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-03-10
Publication Date
2024-10-25
Estimated Expiration
2043-03-10

AI Technical Summary

Technical Problem

Existing monolithic catalysts used to purify VOCs exhaust gas have problems such as low micro-roughness of the carrier, small specific surface area, poor compatibility of active components, high loading rate of precious metals, short service life, and the generation of secondary organic chlorine-containing pollutants, making it difficult to Effective application under complex working conditions.

Method used

Using a carrier-modified catalyst, by improving the original carrier and active components, the solid acid that encapsulates single atoms of precious metals is grafted to improve the mechanical strength of the catalyst and the utilization rate of precious metals, reduce costs, and inhibit the formation of secondary ions through the acid sites of the solid acid. Generation of suborganic chlorine-containing pollutants.

Benefits of technology

It significantly improves the overall performance of the catalyst, expands its application scenarios under complex and harsh working conditions, extends the service life of the catalyst, reduces production costs, and effectively suppresses the generation of toxic secondary pollutants.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present invention provides a carrier-modified catalyst and a preparation method and application thereof. The carrier-modified catalyst comprises a modified carrier and a solid acid encapsulating a single noble metal atom grafted on the surface of the modified carrier. The preparation method comprises: 1) mixing a main carrier, a solid modifier and water, and obtaining a modified carrier through a hydrothermal reaction; 2) mixing the modified carrier with a prepared noble metal precursor mixed solution, and sequentially performing a crystallization reaction and roasting to obtain a molecular sieve catalyst encapsulating a single noble metal atom; 3) reacting the molecular sieve catalyst encapsulating a single noble metal atom with an ammonium nitrate solution, and then roasting to obtain a solid acid catalyst encapsulating a single noble metal atom. The carrier-modified catalyst significantly improves the overall performance of the catalyst by comprehensively improving and optimizing the original carrier and active components, and is widely applicable to the purification treatment of various types of complex organic waste gases, and has good application prospects.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of environmental protection catalysis, and specifically relates to a carrier modified catalyst and a preparation method and application thereof. Background Art

[0002] Volatile Organic Compounds (VOCs) are a common type of industrial waste gas, mainly coming from the pharmaceutical, rubber, plastic, pesticide, dye and other industries. The emission of this type of waste gas can cause serious environmental problems, including ozone pollution and PM2.5 abnormalities. In recent years, with the continuous advancement of green and sustainable development, carrying out engineering construction for VOCs waste gas will be one of the important means to improve the quality of environmental air. Catalytic oxidation is a purification technology that uses catalysts to remove target pollutants in a targeted manner at high temperatures. It has the characteristics of low energy consumption and significant effects. The core of this method lies in the design and development of catalysts with high mechanical strength, good catalytic performance, low price and few secondary pollutants.

[0003] CN113426458A discloses a catalyst for catalytic combustion of halogen-containing volatile organic compounds, the catalyst comprising a monolithic or granular carrier and a high-viscosity coating, an additive and an active component coating loaded on the carrier, wherein the high-viscosity coating is obtained by coating an inorganic oxide carrier with aluminum sol and then calcining the inorganic oxide carrier, and the active component is precipitated on the surface of the high-viscosity coating by a redox method. The catalyst has good stability, regeneration and high moisture resistance, high conversion efficiency for halogen-containing volatile organic compounds, low catalyst preparation cost, and a firm combination of the active coating and the monolithic or granular inorganic oxide carrier.

[0004] However, the integral catalysts currently used to purify VOCs waste gas still face the following challenges: 1) What kind of cheap modifier should be selected to modify the catalyst carrier to overcome the problems of low micro-roughness, small specific surface area, and poor compatibility with active components, so as to expand its application scenarios under complex and harsh working conditions; 2) How to develop an integral catalyst with a low precious metal loading rate while ensuring a high VOCs conversion rate, so as to achieve the goal of reducing catalyst costs; 3) How to avoid the migration, agglomeration, volatilization, loss and poisoning of precious metal species during the reaction, which may cause a decrease in activity, and extend the service life of the catalyst; 4) When treating specific chlorine-containing waste gases, how to inhibit the generation of more toxic and harmful secondary organic chlorine-containing pollutants during the reaction; 5) For different VOCs waste gas working conditions, how to accurately design and prepare high-performance catalysts to avoid the loss of materials and equipment caused by "trial and error".

[0005] In summary, how to develop a catalyst that can solve the above-mentioned problems has become an urgent issue to be solved. Summary of the invention

[0006] In view of the problems existing in the prior art, the purpose of the present invention is to provide a carrier-modified catalyst and a preparation method and application thereof. The carrier-modified catalyst significantly improves the overall performance of the catalyst by comprehensively improving and optimizing the original carrier and active components. It is widely applicable to the purification of various types of complex organic waste gases, especially in the treatment of organic waste gases containing heteroatoms such as Cl, and has significant advantages and good application prospects.

[0007] To achieve this object, the present invention adopts the following technical solutions:

[0008] In a first aspect, the present invention provides a carrier-modified catalyst, the carrier-modified catalyst comprising a modified carrier, and a solid acid encapsulating a single noble metal atom grafted on the surface of the modified carrier;

[0009] The modified carrier includes a main carrier modified by a solid modifier.

[0010] The following are preferred technical solutions of the present invention, but are not intended to be limitations of the technical solutions provided by the present invention. Through the following technical solutions, the technical objectives and beneficial effects of the present invention can be better achieved and realized.

[0011] As a preferred technical solution of the present invention, the main carrier includes cordierite or mullite.

[0012] Preferably, the main components of the solid modifier include Si, O, Al and Mg, and the cost is similar to that of the main carrier.

[0013] Preferably, the solid modifier comprises fly ash.

[0014] As a preferred technical solution of the present invention, the precious metal includes any one of platinum, ruthenium or palladium, or a combination of at least two of them. Typical but non-limiting examples of the combination include: a combination of platinum and ruthenium, a combination of ruthenium and palladium, a combination of platinum, ruthenium and palladium, etc.

[0015] In a second aspect, the present invention provides a method for preparing the carrier-modified catalyst according to the first aspect, the preparation method comprising the following steps:

[0016] (1) mixing a pretreated main carrier, a pretreated solid modifier and water, and performing a hydrothermal reaction to obtain a modified carrier;

[0017] (2) mixing the modified support described in step (1) with the prepared noble metal precursor mixed solution, and sequentially performing crystallization reaction and calcination to obtain a molecular sieve catalyst encapsulating noble metal single atoms;

[0018] (3) reacting the molecular sieve catalyst encapsulating a single noble metal atom described in step (2) with an ammonium nitrate solution, and then calcining the catalyst to obtain a solid acid catalyst encapsulating a single noble metal atom.

[0019] As a preferred technical solution of the present invention, the method for pretreating the main carrier in step (1) comprises: mixing the main carrier with an alkaline solution, performing a hydrothermal reaction, and then washing and drying in sequence to obtain a pretreated main carrier.

[0020] Preferably, the alkaline solution comprises sodium hydroxide solution and / or potassium hydroxide solution.

[0021] Preferably, the concentration of the alkaline solution is 10-20wt%, such as 10wt%, 12wt%, 14wt%, 16wt%, 18wt% or 20wt%, etc., but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0022] Preferably, during the pretreatment of the main carrier, the temperature of the hydrothermal reaction is 120-150°C, for example, 120°C, 125°C, 130°C, 135°C, 140°C, 145°C or 150°C, etc.; the time is 10-16h, for example, 10h, 12h, 14h or 16h, etc., but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0023] As a preferred technical solution of the present invention, the method for pretreating the solid modifier in step (1) comprises: sequentially acid-washing and drying the solid modifier, mixing it with an alkaline substance, and then grinding and roasting it to obtain a pretreated solid modifier.

[0024] Preferably, the acid solution used for pickling includes hydrochloric acid.

[0025] Preferably, the concentration of the hydrochloric acid is 1-10mol / L, for example 10mol / L, 10mol / L, 10mol / L, 10mol / L, 10mol / L, 10mol / L or 10mol / L, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0026] Preferably, the mass ratio of the solid modifier to the acid solution is 1:(1-10), such as 1:1, 1:2, 1:4, 1:6, 1:8 or 1:10, etc., but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0027] Preferably, the alkaline substance includes any one of sodium hydroxide, sodium carbonate, potassium hydroxide or potassium carbonate, or a combination of at least two of them. Typical but non-limiting examples of the combination include a combination of sodium hydroxide and potassium hydroxide, and a combination of sodium carbonate and potassium carbonate.

[0028] Preferably, the mass ratio of the solid modifier to the alkaline substance is 1:(0.5-3), such as 1:0.5, 1:1, 1:1.5, 1:2, 1:2.5 or 1:3, etc., but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0029] Preferably, during the pretreatment of the solid modifier, the calcination temperature is 400-900°C, for example, 400°C, 500°C, 600°C, 700°C, 800°C or 900°C, etc.; the time is 1-5h, for example, 1h, 2h, 3h, 4h or 5h, etc. The selection of the above numerical values ​​is not limited to the listed values, and other unlisted values ​​within the respective numerical ranges are also applicable.

[0030] As a preferred technical solution of the present invention, the mass ratio of the pretreated solid modifier to water in step (1) is 1:(2-20), for example 1:2, 1:4, 1:6, 1:8, 1:10, 1:12, 1:14, 1:18 or 1:20, etc., but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0031] Preferably, the temperature of the hydrothermal reaction in step (1) is 80-200°C, for example 80°C, 100°C, 120°C, 160°C, 180°C or 200°C, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0032] Preferably, the time of the hydrothermal reaction in step (1) is 4-24 h, for example 4 h, 8 h, 12 h, 16 h, 20 h or 24 h, etc., but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0033] As a preferred technical solution of the present invention, the method for preparing the noble metal precursor mixed solution in step (2) includes: mixing the noble metal precursor, an organic nitrogen-containing ligand, a template, an aluminum source, sodium hydroxide, a silicon source and water to obtain the noble metal precursor mixed solution.

[0034] Preferably, the noble metal precursor and the organic nitrogen-containing ligand are first fully dissolved and mixed, and then the template, the aluminum source and sodium hydroxide are added, followed by slowly adding the silicon source, and a mixed solution is obtained after vigorous stirring.

[0035] Preferably, the molar ratio of the noble metal precursor to the organic nitrogen-containing ligand is 1:(20-50), for example 1:20, 1:25, 1:30, 1:35, 1:40, 1:45 or 1:50, etc., but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0036] Preferably, the molar ratio of the aluminum source, water, sodium hydroxide, template and silicon source is 1:(100-1000):(1-10):(5-200):(10-50), for example 1:100:1:5:10, 1:200:4:40:30, 1:400:7:100:40, 1:300:2:200:50 or 1:100:10:180:12, etc., but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0037] Preferably, the molar ratio of the noble metal precursor to the water is 1:(20000-80000), for example 1:20000, 1:30000, 1:40000, 1:50000, 1:60000, 1:70000 or 1:80000, etc., but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0038] Preferably, the noble metal precursor includes any one of chloroplatinic acid, platinum nitrate, tetraamineplatinum nitrate, ruthenium nitrate, ruthenium chloride, palladium chloride, palladium nitrate or tetraaminepalladium nitrate, or a combination of at least two thereof. Typical but non-limiting examples of the combination include: a combination of chloroplatinic acid and platinum nitrate, a combination of chloroplatinic acid and ruthenium chloride, a combination of ruthenium chloride and palladium chloride, etc.

[0039] Preferably, the organic nitrogen-containing ligand comprises ethylenediamine and / or diethylenetriamine.

[0040] Preferably, the template comprises any one of N,N,N-trimethyl-1-adamantane-ammonium hydroxide, tetraethylammonium hydroxide, tetrapropylammonium hydroxide or choline chloride, or a combination of at least two thereof. Typical but non-limiting examples of the combination include a combination of N,N,N-trimethyl-1-adamantane-ammonium hydroxide and tetraethylammonium hydroxide, a combination of tetraethylammonium hydroxide and tetrapropylammonium hydroxide, and the like.

[0041] Preferably, the aluminum source includes any one of sodium aluminate, aluminum sulfate, aluminum nitrate or aluminum isopropoxide, or a combination of at least two thereof. Typical but non-limiting examples of the combination include a combination of sodium aluminate and aluminum sulfate, a combination of aluminum sulfate and aluminum nitrate, and the like.

[0042] Preferably, the silicon source includes any one of white carbon black, tetraethyl orthosilicate, silica sol or methyl orthosilicate, or a combination of at least two thereof. Typical but non-limiting examples of the combination include a combination of tetraethyl orthosilicate and silica sol.

[0043] Preferably, the temperature of the crystallization reaction in step (2) is 120-200°C, for example, 120°C, 140°C, 160°C, 180°C or 200°C, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0044] Preferably, the crystallization reaction time in step (2) is 72-200 h, for example 72 h, 80 h, 90 h, 100 h, 120 h, 140 h, 180 h or 200 h, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0045] Preferably, the calcination temperature in step (2) is 450-650°C, for example 450°C, 500°C, 550°C, 600°C or 650°C, but is not limited to the listed values, and other values ​​not listed within the range are also applicable.

[0046] Preferably, the calcination time in step (2) is 2-8 h, for example 2 h, 3 h, 4 h, 5 h, 6 h, 7 h or 8 h, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0047] As a preferred technical solution of the present invention, the concentration of the ammonium nitrate solution in step (3) is 2-3 mol / / L, for example, 2 mol / / L, 2.2 mol / / L, 2.4 mol / / L, 2.6 mol / / L, 2.8 mol / / L or 3 mol / / L, etc., but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0048] Preferably, the reaction temperature in step (3) is 70-80°C, such as 70°C, 72°C, 74°C, 76°C, 78°C or 80°C, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0049] Preferably, the reaction time of step (3) is 2-6 h, such as 2 h, 3 h, 4 h, 5 h or 6 h, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0050] Preferably, the calcination temperature in step (3) is 450-650°C, for example 450°C, 500°C, 550°C, 600°C or 650°C, but is not limited to the listed values, and other values ​​not listed within the range are also applicable.

[0051] Preferably, the calcination time in step (3) is 1-8 h, for example, 1 h, 2 h, 3 h, 4 h, 5 h, 6 h, 7 h or 8 h, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0052] In a third aspect, the present invention provides a use of the carrier-modified catalyst described in the first aspect, wherein the carrier-modified catalyst is used for purifying VOCs.

[0053] Compared with the prior art, the present invention has the following beneficial effects:

[0054] (1) Compared with the original catalyst carrier, the carrier-modified catalyst of the present invention uses a solid modifier with a component close to that of the carrier to modify the catalyst surface, which can significantly increase the micro-roughness and specific surface area of ​​the carrier, and is helpful for the subsequent in-situ grafting of the solid acid encapsulating the noble metal single atom on the surface of the modified carrier, thereby solving the problems of poor compatibility between the active component and the carrier, high coating slurry loss, and high coating shedding rate in the preparation of monolithic catalysts by the traditional wet coating production process, improving the mechanical strength of the monolithic catalyst, and expanding the application scenarios of the catalyst under complex and harsh working conditions such as high humidity and high space velocity;

[0055] (2) Compared with the traditional noble metal nanoparticle catalyst, the noble metal single atom catalyst of the present invention has a unique valence electron structure and an ideal noble metal utilization rate, which can reduce the noble metal loading rate on the basis of ensuring a high VOCs conversion rate, thereby achieving the purpose of reducing the catalyst cost; on the other hand, the noble metal is encapsulated in the solid acid in the form of a single atom dispersion, which can not only inhibit its migration and agglomeration in a high temperature environment, but also avoid the volatilization, loss and poisoning of the noble metal, thereby ensuring the purification stability of the catalyst and extending the service life of the catalyst;

[0056] (3) The solid acid catalyst surface of the present invention has a large amount of Acid sites can provide enough protons to combine with chlorine to generate HCl when treating chlorinated VOCs under special working conditions, avoiding the generation of highly reactive and oxidizing Cl2 during the reaction, thereby inhibiting the generation of more toxic and harmful secondary organic chlorinated pollutants;

[0057] (4) The present invention establishes a target-oriented strategy of "operating conditions-precious metal combination-catalyst" to achieve the purpose of accurately designing high-performance catalysts for use under complex exhaust gas conditions. DETAILED DESCRIPTION

[0058] In order to better illustrate the present invention and facilitate understanding of the technical solution of the present invention, the present invention is further described in detail below. However, the following embodiments are only simple examples of the present invention and do not represent or limit the scope of protection of the present invention. The scope of protection of the present invention shall be subject to the claims.

[0059] The following are typical but non-limiting embodiments of the present invention:

[0060] Embodiment 1:

[0061] This embodiment provides a method for preparing a carrier-modified catalyst, the preparation method comprising the following steps:

[0062] S101, repeatedly washing the main carrier (honeycomb cordierite) with deionized water and drying, then transferring the main carrier and a 10 wt% sodium hydroxide solution to a hydrothermal reactor, reacting at 120° C. for 14 h, and after the reaction is completed, washing and drying to obtain a pretreated carrier;

[0063] S102, fly ash is mixed with 5 mol / L hydrochloric acid solution at a mass ratio of 1:5, and then stirred, filtered and dried in sequence to obtain a dry product; the dry product is mixed with sodium hydroxide at a mass ratio of 1:1, ground, and then roasted at 800°C for 3h to obtain pretreated fly ash; then the pretreated fly ash is mixed with deionized water at a mass ratio of 1:5 and stirred to obtain a first mixed solution; the first mixed solution and the pretreated carrier in step (1) are transferred to a hydrothermal reactor, reacted at 120°C for 15h, and after the reaction is completed, washed and dried to obtain a fly ash modified carrier;

[0064] S103, chloroplatinic acid, ethylenediamine, and deionized water are mixed and stirred in a molar ratio of 1:25:20000, and then tetrapropylammonium hydroxide, sodium aluminate, and sodium hydroxide are added for ultrasonic stirring, and then tetraethyl orthosilicate is slowly added and vigorously stirred to obtain a second mixed solution (wherein the molar ratio of sodium aluminate to tetraethyl orthosilicate, deionized water, sodium hydroxide, and tetrapropylammonium hydroxide is 1:10:200:3:30); then the second mixed solution and the fly ash modified carrier are transferred to a reactor with a polytetrafluoroethylene liner, crystallized at 150°C for 98h, and after the reaction is completed, washed and dried, and calcined at 550°C for 5h to obtain a molecular sieve catalyst encapsulating a single platinum atom;

[0065] S104, transferring the prepared molecular sieve catalyst encapsulating single platinum atoms to a 2 mol / L ammonium nitrate solution, reacting it at 80°C for 3 hours, washing and drying it, and then calcining it at 550°C for 5 hours to obtain a solid acid catalyst encapsulating single platinum atoms.

[0066] In the solid acid catalyst encapsulating platinum atoms obtained in this example, the shedding rate of the coating on the carrier surface was 0.5 wt %. -1 Under the space velocity condition, the purification efficiency of toluene reaches 99% at 330℃; after running at 350℃ for 20h, the activity of the obtained catalyst decreases by 0.5%.

[0067] Comparative Example 1:

[0068] This comparative example provides a method for preparing a carrier-modified catalyst. The preparation method refers to the preparation method in Example 1, with the only difference being that step S102 is not performed, that is, the main carrier is not modified with fly ash, and the rest remains unchanged.

[0069] In the solid acid catalyst encapsulating platinum atoms obtained in this comparative example, the shedding rate of the coating on the carrier surface reached 10.3wt%. -1 Under the space velocity conditions, the purification efficiency of toluene reached 99% at 360℃; after running at 350℃ for 20h, the activity decreased by 5.1%.

[0070] Embodiment 2:

[0071] This embodiment provides a method for preparing a carrier-modified catalyst, the preparation method comprising the following steps:

[0072] S101, repeatedly washing the main carrier (honeycomb mullite) with deionized water and drying, then transferring the main carrier and a 10 wt% potassium hydroxide solution to a hydrothermal reactor, reacting at 130° C. for 11 h, and after the reaction is completed, washing and drying to obtain a pretreated carrier;

[0073] S102, mixing fly ash with 5 mol / L hydrochloric acid solution at a mass ratio of 1:5, then stirring, filtering and drying in sequence to obtain a dry product; mixing the dry product with sodium hydroxide at a mass ratio of 1:1, grinding, and then roasting at 700°C for 4 hours to obtain pretreated fly ash; then mixing the pretreated fly ash with deionized water at a mass ratio of 1:5, stirring to obtain a first mixed solution; transferring the first mixed solution and the pretreated carrier in step (1) to a hydrothermal reactor, reacting at 150°C for 12 hours, and washing and drying after the reaction to obtain a fly ash modified carrier;

[0074] S103, palladium nitrate, ethylenediamine, and deionized water are mixed and stirred in a molar ratio of 1:25:30000, and then tetrapropylammonium hydroxide, sodium aluminate, and sodium hydroxide are added for ultrasonic stirring, and then tetraethyl orthosilicate is slowly added and vigorously stirred to obtain a second mixed solution (wherein the molar ratio of sodium aluminate to tetraethyl orthosilicate, deionized water, sodium hydroxide, and tetrapropylammonium hydroxide is 1:10:300:3:40); then the second mixed solution and the fly ash modified carrier are transferred to a reactor with a polytetrafluoroethylene liner, crystallized at 130° C. for 120 h, and after the reaction is completed, washed and dried, and calcined at 600° C. for 4 h to obtain a molecular sieve catalyst encapsulating a palladium single atom;

[0075] S104, transferring the prepared molecular sieve catalyst encapsulating a single palladium atom to a 2 mol / L ammonium nitrate solution, and reacting it at 80°C for 3 hours, and then washing and drying it, and calcining it at 550°C for 5 hours to obtain a solid acid catalyst encapsulating a single palladium atom.

[0076] In the solid acid catalyst encapsulating palladium atoms obtained in this example, the shedding rate of the coating on the surface of the carrier was 0.6 wt %. -1 Under the space velocity conditions, the purification efficiency of chlorobenzene reached 99% at 427℃; after running at 500℃ for 20h, the activity of the obtained catalyst decreased by 0.4%.

[0077] Comparative Example 2:

[0078] This comparative example provides a method for preparing a carrier-modified catalyst. The preparation method refers to the preparation method in Example 2, with the only difference being that in S103, the dosage of palladium nitrate and ethylenediamine is increased to 40 times, i.e., the molar ratio of palladium nitrate, ethylenediamine, and deionized water is 40:1000:30000, and other conditions remain unchanged, thereby obtaining a solid acid catalyst encapsulating palladium nanoparticles.

[0079] In the solid acid catalyst encapsulated with palladium nanoparticles obtained in this comparative example, the shedding rate of the coating on the surface of the carrier reached 1.5wt%. -1 Under the space velocity conditions, the purification efficiency of chlorobenzene reached 99% at 435℃; after running at 500℃ for 20h, the activity decreased by 4.5%.

[0080] Embodiment 3:

[0081] This embodiment provides a method for preparing a carrier-modified catalyst, the preparation method comprising the following steps:

[0082] S101, repeatedly washing the main carrier (honeycomb cordierite) with deionized water and drying, then transferring the main carrier and a 10 wt% sodium hydroxide solution to a hydrothermal reactor, reacting at 120° C. for 14 h, and after the reaction is completed, washing and drying to obtain a pretreated carrier;

[0083] S102, fly ash is mixed with 5 mol / L hydrochloric acid solution at a mass ratio of 1:5, and then stirred, filtered and dried in sequence to obtain a dry product; the dry product is mixed with sodium hydroxide at a mass ratio of 1:1, ground, and then roasted at 800°C for 3h to obtain pretreated fly ash; then the pretreated fly ash is mixed with deionized water at a mass ratio of 1:5 and stirred to obtain a first mixed solution; the first mixed solution and the pretreated carrier in step (1) are transferred to a hydrothermal reactor, reacted at 120°C for 15h, and after the reaction is completed, washed and dried to obtain a fly ash modified carrier;

[0084] S103, ruthenium chloride, ethylenediamine, diethylenetriamine, and deionized water are mixed and stirred in a molar ratio of 1:20:20:50000, and then tetrapropylammonium hydroxide, sodium aluminate, and sodium hydroxide are added for ultrasonic stirring, and then tetraethyl orthosilicate is slowly added and vigorously stirred to obtain a second mixed solution (wherein the molar ratio of sodium aluminate to tetraethyl orthosilicate, deionized water, sodium hydroxide, and tetrapropylammonium hydroxide is 1:10:600:6:50); then the second mixed solution and the fly ash modified carrier are transferred to a reactor with a polytetrafluoroethylene liner, crystallized at 160°C for 110h, and after the reaction is completed, washed and dried, and calcined at 550°C for 4h to obtain a molecular sieve catalyst encapsulating a single ruthenium atom;

[0085] S104, transferring the prepared molecular sieve catalyst encapsulating single ruthenium atoms to a 2 mol / L ammonium nitrate solution, and reacting it at 80°C for 3 hours, and then washing and drying it, and calcining it at 550°C for 5 hours to obtain a solid acid catalyst encapsulating single ruthenium atoms.

[0086] In the solid acid catalyst encapsulating ruthenium single atoms obtained in this example, the shedding rate of the coating on the support surface was 0.4 wt %. -1 Under the space velocity conditions, the purification efficiency of chlorobenzene reaches 99% at 425℃; in the range of 400-500℃, the selectivity of HCl is >85%, and after running at 500℃ for 20h, the activity decreases by 0.2%.

[0087] Comparative Example 3:

[0088] This comparative example provides a method for preparing a carrier-modified catalyst. The preparation method refers to the preparation method in Example 3, with the only difference being that S104 is not performed, and the rest is the same.

[0089] In the molecular sieve catalyst encapsulating ruthenium single atoms obtained in this comparative example, the shedding rate of the coating on the carrier surface reached 1.1wt%. -1 Under the space velocity conditions, the purification efficiency of chlorobenzene reached 99% at 439°C; in the range of 400-500°C, the selectivity of HCl was <50%, and after running at 500°C for 20 hours, the activity decreased by 3.2%.

[0090] Embodiment 4:

[0091] This embodiment provides a method for preparing a carrier-modified catalyst, which refers to the preparation method in Example 1, with the only difference being that in S103, when preparing the second mixed solution, chloroplatinic acid, ruthenium nitrosyl nitrate, ethylenediamine, and deionized water are mixed in a molar ratio of 0.5:0.5:25:30000, that is, two precious metal precursors are introduced, and the rest remain unchanged.

[0092] In the solid acid catalyst encapsulating platinum / ruthenium single atoms obtained in this example, the shedding rate of the coating on the carrier surface was 0.3wt%. -1 Under the space velocity condition, the purification efficiency of dichloromethane reaches 99% at 411℃.

[0093] Embodiment 5:

[0094] This embodiment provides a method for preparing a carrier-modified catalyst, which refers to the preparation method in Example 2, with the only difference being that in S103, when preparing the second mixed solution, palladium nitrate, ruthenium chloride, ethylenediamine, and deionized water are mixed in a molar ratio of 0.4:0.6:30:30000, that is, two precious metal precursors are introduced, and the rest remain unchanged.

[0095] In the solid acid catalyst encapsulating palladium / ruthenium single atoms obtained in this example, the shedding rate of the coating on the surface of the carrier is 0.65wt%. -1 Under the space velocity conditions, the purification efficiency of trichloroethylene reaches 99% at 395℃.

[0096] It can be seen from the above embodiments and comparative examples that the carrier-modified catalyst of the present invention significantly improves the overall performance of the catalyst by comprehensively improving and optimizing the original carrier and active components, and is widely applicable to the purification of various complex organic waste gases, especially in the treatment of organic waste gases containing heteroatoms such as Cl, and has significant advantages and good application prospects.

[0097] The present invention illustrates the products and detailed methods of the present invention through the above embodiments, but the present invention is not limited to the above products and detailed methods, that is, it does not mean that the present invention must rely on the above products and detailed methods to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of the operation of the present invention, addition of auxiliary operations, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.

Claims

1. A carrier-modified catalyst, characterized in that: The carrier-modified catalyst comprises a modified carrier and a solid acid encapsulating a single noble metal atom grafted on the surface of the modified carrier; The modified carrier includes a main carrier modified by a solid modifier; The main carrier includes cordierite or mullite; the solid modifier includes fly ash; The carrier-modified catalyst is prepared by the following method, which comprises the following steps: (1) mixing a pretreated main carrier, a pretreated solid modifier and water, and performing a hydrothermal reaction to obtain a modified carrier; (2) mixing the modified support described in step (1) with the prepared noble metal precursor mixed solution, and sequentially performing crystallization reaction and calcination to obtain a molecular sieve catalyst encapsulating noble metal single atoms; The method for preparing the noble metal precursor mixed solution comprises: mixing the noble metal precursor, an organic nitrogen-containing ligand, a template, an aluminum source, sodium hydroxide, a silicon source and water to obtain the noble metal precursor mixed solution; (3) reacting the molecular sieve catalyst encapsulating a single noble metal atom described in step (2) with an ammonium nitrate solution, and then calcining the catalyst to obtain a solid acid catalyst encapsulating a single noble metal atom.

2. The carrier-modified catalyst according to claim 1, characterized in that: The noble metal includes any one of platinum, ruthenium or palladium, or a combination of at least two of them.

3. A method for preparing a carrier-modified catalyst as claimed in claim 1 or 2, characterized in that: The preparation method comprises the following steps: (1) mixing a pretreated main carrier, a pretreated solid modifier and water, and performing a hydrothermal reaction to obtain a modified carrier; (2) mixing the modified support described in step (1) with the prepared noble metal precursor mixed solution, and sequentially performing crystallization reaction and calcination to obtain a molecular sieve catalyst encapsulating noble metal single atoms; The method for preparing the noble metal precursor mixed solution comprises: mixing the noble metal precursor, an organic nitrogen-containing ligand, a template, an aluminum source, sodium hydroxide, a silicon source and water to obtain the noble metal precursor mixed solution; (3) reacting the molecular sieve catalyst encapsulating a single noble metal atom described in step (2) with an ammonium nitrate solution, and then calcining the catalyst to obtain a solid acid catalyst encapsulating a single noble metal atom.

4. The method for preparing a carrier-modified catalyst according to claim 3, characterized in that: The method for pretreating the main carrier in step (1) comprises: mixing the main carrier with an alkaline solution, performing a hydrothermal reaction, and then washing and drying in sequence to obtain a pretreated main carrier.

5. The method for preparing a carrier-modified catalyst according to claim 4, characterized in that: The alkaline solution includes sodium hydroxide solution and / or potassium hydroxide solution.

6. The method for preparing a carrier-modified catalyst according to claim 4, characterized in that: The concentration of the alkaline solution is 10-20 wt%.

7. The method for preparing a carrier-modified catalyst according to claim 4, characterized in that: During the pretreatment of the main carrier, the temperature of the hydrothermal reaction is 120-150° C. and the time is 10-16 hours.

8. The method for preparing a carrier-modified catalyst according to claim 3, characterized in that: The method for pretreating the solid modifier in step (1) comprises: sequentially acid-washing and drying the solid modifier, mixing it with an alkaline substance, and then grinding and roasting it to obtain a pretreated solid modifier.

9. The method for preparing a carrier-modified catalyst according to claim 8, characterized in that: The acid solution used in the pickling includes hydrochloric acid.

10. The method for preparing a carrier-modified catalyst according to claim 9, characterized in that: The concentration of the hydrochloric acid is 1-10 mol / L.

11. The method for preparing a carrier-modified catalyst according to claim 8, characterized in that: The mass ratio of the solid modifier to the acid solution is 1:(1-10).

12. The method for preparing a carrier-modified catalyst according to claim 8, characterized in that: The alkaline substance includes any one of sodium hydroxide, sodium carbonate, potassium hydroxide or potassium carbonate, or a combination of at least two thereof.

13. The method for preparing a carrier-modified catalyst according to claim 8, characterized in that: The mass ratio of the solid modifier to the alkaline substance is 1:(0.5-3).

14. The method for preparing a carrier-modified catalyst according to claim 8, characterized in that: During the pretreatment of the solid modifier, the calcination temperature is 400-900° C. and the calcination time is 1-5 hours.

15. The method for preparing a carrier-modified catalyst according to claim 3, characterized in that: The mass ratio of the pretreated solid modifier to water in step (1) is 1:(2-20).

16. The method for preparing a carrier-modified catalyst according to claim 3, characterized in that: The temperature of the hydrothermal reaction in step (1) is 80-200°C.

17. The method for preparing a carrier-modified catalyst according to claim 3, characterized in that: The time of the hydrothermal reaction in step (1) is 4-24 hours.

18. The preparation method according to claim 3, characterized in that: In step (2), the molar ratio of the noble metal precursor to the organic nitrogen-containing ligand is 1:(20-50).

19. The preparation method according to claim 3, characterized in that: The molar ratio of the aluminum source, water, sodium hydroxide, template and silicon source in step (2) is 1:(100-1000):(1-10):(5-200):(10-50).

20. The preparation method according to claim 3, characterized in that: In step (2), the molar ratio of the noble metal precursor to the water is 1:(20000-80000).

21. The preparation method according to claim 3, characterized in that: The noble metal precursor in step (2) includes any one of chloroplatinic acid, platinum nitrate, tetraammineplatinum nitrate, nitrosylruthenium nitrate, ruthenium chloride, palladium chloride, palladium nitrate or tetraamminepalladium nitrate, or a combination of at least two thereof.

22. The preparation method according to claim 3, characterized in that: The organic nitrogen-containing ligand in step (2) includes ethylenediamine and / or diethylenetriamine.

23. The preparation method according to claim 3, characterized in that: The template in step (2) includes any one of N,N,N-trimethyl-1-adamantane-ammonium hydroxide, tetraethylammonium hydroxide, tetrapropylammonium hydroxide or choline chloride, or a combination of at least two thereof.

24. The preparation method according to claim 3, characterized in that: The aluminum source in step (2) includes any one of sodium aluminate, aluminum sulfate, aluminum nitrate or aluminum isopropoxide, or a combination of at least two of them.

25. The preparation method according to claim 3, characterized in that: The silicon source in step (2) includes any one of white carbon black, ethyl orthosilicate, silica sol or methyl orthosilicate, or a combination of at least two of them.

26. The preparation method according to claim 3, characterized in that: The temperature of the crystallization reaction in step (2) is 120-200°C.

27. The preparation method according to claim 3, characterized in that: The crystallization reaction time in step (2) is 72-200h.

28. The preparation method according to claim 3, characterized in that: The calcination temperature in step (2) is 450-650°C.

29. The preparation method according to claim 3, characterized in that: The calcination time in step (2) is 2-8 hours.

30. The preparation method according to claim 3, characterized in that: The concentration of the ammonium nitrate solution in step (3) is 2-3 mol / / L.

31. The preparation method according to claim 3, characterized in that: The reaction temperature in step (3) is 70-80°C.

32. The preparation method according to claim 3, characterized in that: The reaction time of step (3) is 2-6h.

33. The preparation method according to claim 3, characterized in that: The calcination temperature in step (3) is 450-650°C.

34. The preparation method according to claim 3, characterized in that: The calcination time in step (3) is 1-8h.

35. A use of a carrier-modified catalyst as claimed in claim 1 or 2, characterized in that: The carrier-modified catalyst is used for purifying VOCs.