A method for improving the billet forming rate at the end of continuous casting of large-size round billets
By reducing the pulling speed of the tail furnace and adjusting the electromagnetic stirring parameters, the problem of poor internal quality of the continuous cast round billet is solved, the billet yield and efficiency are improved, the scrapped tail billet can be cut into qualified billets, and the production cost is reduced.
Patent Information
- Application Number
- CN202211547336.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-05
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2042-12-05
AI Technical Summary
The internal quality defects of continuous cast round billets lead to low productivity, low billet yield and high production costs. In particular, the internal quality of the tail billet is poor, which affects the billet yield.
By reducing the pulling speed of the tail furnace, adjusting the specific water content and the terminal electromagnetic stirring current and frequency, the width of the liquid phase cavity is increased and the length is shortened, the convection of molten steel is strengthened, poor feeding of molten steel is improved, the growth of columnar crystals and broken dendrite bridging are inhibited, and the central solidification is improved. organize.
It improves the yield rate of continuous cast round billets and reduces quality objections caused by internal defects, allowing scrap tail billets to be cut into qualified billets and scrap billets, reducing production costs and increasing company benefits.
Smart Images

Figure CN116329509B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of special steel, relates to improving the internal quality of large-size continuous casting round billets with a diameter of 450 mm to 800 mm at the end of casting, and specifically relates to a method for improving the billet forming rate at the end of casting of large-size continuous casting round billets. Background Art
[0002] The quality defects of continuous casting billets will affect the productivity, billet yield, final use performance and production cost of the billets. The internal quality of the tail billet is often poor, and due to poor shrinkage compensation of the molten steel, it is often accompanied by serious central looseness, which seriously affects the billet yield of the continuous casting round billet. Therefore, in the continuous casting process, how to improve the internal quality of the tail billet, shorten the length of the scrapped tail billet and thus increase the billet yield is very important. This will not only improve the internal quality of the tail billet, but also further reduce production costs and increase company benefits.
[0003] During continuous casting, the main factor affecting the internal quality of the ingot is the movement state of the molten steel during the solidification process. Due to the dendrite bridging, the molten steel at the end of solidification is not well compensated, resulting in looseness and shrinkage holes inside the ingot. Reducing the casting speed can shorten the length of the liquid phase hole and improve the shortcomings of poor molten steel shrinkage compensation, thereby achieving the purpose of improving the internal quality of the ingot.
[0004] The electromagnetic stirring technology is to strengthen the flow of molten steel in the liquid phase hole by means of the electromagnetic force induced in the liquid phase hole of the ingot, thereby strengthening the convection, heat transfer and mass transfer process of the molten steel, and thus controlling the solidification process of the ingot. This method uses M-EMS and F-EMS combined stirring, which can achieve the following metallurgical effects: disperse the aggregation of solute elements in the two-phase region of solidification, reduce central segregation; improve the central solidification structure, reduce central looseness; eliminate the V-type segregation caused by the slip and collapse of the central equiaxed crystal region. However, in order to achieve a better stirring effect, it is also necessary to consider the accurate installation position of the stirrer, which must be in the two-phase region at the end of the solidification of the ingot; the power of the stirrer should be large enough to rotate the high-viscosity molten steel in the paste zone; the pulling speed and secondary cooling should be stable and controllable; implement alternating stirring, regularly change the flow direction of the molten steel, and inhibit the formation of V-type segregation and white bright bands. Summary of the invention
[0005] The present invention aims at the deficiencies in the prior art and provides a method for improving the billet formation rate at the end of continuous casting of large-size round billets. The method increases the width of the liquid phase hole and shortens the length, strengthens the molten steel convection, improves the shortcomings of poor shrinkage compensation of the molten steel in the casting billet, inhibits the growth of columnar crystals, breaks dendrites, bridges, improves the central solidification structure, and reduces looseness. It not only improves the internal quality of the last furnace billet, reduces the quality objections caused by internal defects, but also increases the billet formation rate of the continuous casting round billet and increases the benefits. Specifically, the original scrapped tail billets can be cut into scrapped billets and qualified billets. The original scrapped tail billets are whole billets. For example, the original specification of ∅450mm-∅600mm round billets with a scrapped whole billet length of 6.0m-6.5m are first cut to form scrapped billets of 3-3.5m and qualified billets of 3.0m-3.5m. The original ∅700mm-∅800mm scrapped whole billet length of 5.5m-6.0m is cut to form scrapped billets of 3-3.5m and qualified billets of 2.5m-3m.
[0006] The technical solution disclosed in the present invention is as follows: a method for improving the billet forming rate at the end of continuous casting of large-sized round billets,
[0007] Reduce the pulling speed for the last package in the middle package;
[0008] Adjust F-EMS current and specific water volume simultaneously;
[0009] The tail billet cutting is divided into qualified billets and scrap billets.
[0010] On the basis of the above scheme, as a preferred embodiment, the pulling speed of the last bag of the middle bag is reduced by 0.04-0.1m / min, the F-EMS current is reduced by 10-15A, and the specific water content is adjusted from 0.005L / kg to 0.02L / kg.
[0011] On the basis of the above scheme, as a preferred option, for 4130X-12 round billets with ∅450-∅600, the pulling speed of the last package of the tundish is reduced from 0.33m / min to 0.23m / min, the F-EMS current is reduced from 90A to 80A, and the specific water content is adjusted from 0.095L / kg to 0.080L / kg.
[0012] Based on the above scheme, as a preferred method, for A105 / LF2 round billets with ∅450-∅600, the pulling speed of the last package of the tundish is reduced from 0.45m / min to 0.35m / min, the F-EMS current is adjusted from 125A to 110A, and the specific water content is adjusted from 0.111L / kg to 0.100L / kg.
[0013] On the basis of the above scheme, as a preferred option, for 30Mn2 round billets with ∅700-∅800, the pulling speed of the last package of the tundish is reduced from 0.24m / min to 0.18m / min, the F-EMS current is adjusted from 240A to 220A, and the specific water content is adjusted from 0.071L / kg to 0.066L / kg.
[0014] On the basis of the above scheme, as a preferred embodiment, the tail billet is cut into scrap billets with a length of 3-3.5 m, and the remaining finished billets are finished billets.
[0015] Compared with the prior art, the present invention has the following beneficial effects:
[0016] By reducing the tail furnace pulling speed, adjusting the specific water volume, and adjusting the terminal electromagnetic stirring current and frequency, the liquid phase hole width can be increased, the length can be shortened, and the molten steel convection can be strengthened, thereby improving the shortcomings of poor shrinkage compensation of molten steel in the ingot.
[0017] Inhibit the growth of columnar crystals, break up dendrites and bridge to improve the central solidification structure, disperse the aggregation of solute elements in the two phases of solidification, reduce central segregation, reduce central porosity, and eliminate V-type segregation caused by slip and collapse of the central equiaxed crystal zone.
[0018] It not only improves the internal quality of the last furnace tail billet and reduces the quality objections caused by internal defects, but also increases the billet formation rate of continuous casting round billets and increases benefits.
[0019] The original scrapped tail billets can be cut into scrapped billets and qualified billets. The original scrapped tail billets are whole billets. For example, the original specification of ∅450mm-∅600mm round billets with a scrapped whole billet length of 6.0m-6.5m are first cut to form scrapped billets of 3-3.5m and qualified billets of 3.0m-3.5m. The original ∅700mm-∅800mm scrapped whole billet length of 5.5m-6.0m is cut to form scrapped billets of 3-3.5m and qualified billets of 2.5m-3m.
[0020] Improved the output of finished products. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 This is the picture of the tail of sample 1 at 4.0m;
[0022] Figure 2 This is the picture of the tail of sample 1 at 3.5m;
[0023] Figure 3 This is the picture of the tail of sample 1 at 3.0m;
[0024] Figure 4 This is the picture of the tail of sample 1 at 2.5m;
[0025] Figure 5 This is the picture of the tail of sample 2 at 4.0m;
[0026] Figure 6 This is the picture of the tail of sample 2 at 3.5m;
[0027] Figure 7 This is the picture of the tail of sample 2 at 3.0m;
[0028] Figure 8 This is the picture of the tail of sample 2 at 2.5m;
[0029] Fig. 9 This is the picture of the tail of sample 3 at 4.0m;
[0030] Fig.10 This is the picture of the tail of sample 3 at 3.5m;
[0031] Fig.11 This is the picture of the tail of sample 3 at 3.0m;
[0032] Fig.12 This is the picture of the tail of sample 3 at 2.5m;
[0033] Fig.13 This is the picture of the tail of specimen 4 at 4.0m;
[0034] Fig.14 This is the picture of the tail of specimen 4 at 3.5m;
[0035] Fig.15 This is the picture of the tail of specimen 4 at 3.0m;
[0036] Fig.16 This is the picture of the tail of sample 4 at 2.5m;
[0037] Fig.17 This is the picture of the tail of specimen 5 at 4.0m;
[0038] Fig.18 This is the picture of the tail of specimen 5 at 3.5m;
[0039] Fig.19 This is the picture of the tail of sample 5 at 3.0m;
[0040] Fig. 20 This is a picture of the sample 5 at 2.5m from the tail. DETAILED DESCRIPTION
[0041] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the specific implementation methods of the present invention will be described below with reference to the accompanying drawings. Obviously, the accompanying drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings and other implementation methods can be obtained based on these drawings without creative work.
[0042] Continuous casting large-size round billet pouring process: In the middle of LF refining, after the alloy composition is adjusted to the target value, the temperature begins to rise to ensure the superheat of the continuous casting molten steel. After vacuum treatment, it is promptly sent to the continuous casting for pouring to ensure the smooth continuous casting pouring.
[0043] In the process of power transmission and refining, add appropriate amount of slag surface deoxidation, control the white slag time ≥ 20 minutes, and do not add any materials 5 minutes before leaving the station.
[0044] During the electrode power-on heating process, the temperature of the first ladle rises to the liquidus temperature +70℃-90℃, and the temperature of the continuous casting furnace rises to the liquidus temperature +50℃-80℃; the continuous casting overheating is controlled at 15℃-35℃; for the molten steel that has passed the vacuum, the vacuum treatment station must ensure that the next ladle is hoisted to the continuous casting platform within 2 minutes before the previous molten steel is poured.
[0045] After the ladle arrives at the platform, the ladle cover should be covered in time. After the ladle starts pouring, the temperature should be measured manually first, and the second ladle should be put into use for continuous temperature measurement. At the same time, each ladle needs to be calibrated manually to ensure the normal use of continuous temperature measurement and the accuracy of superheat.
[0046] in,
[0047] Before the ladle starts pouring, insert the argon blowing tube into the long water nozzle and adjust the flow rate to 40L / min; after the tundish baking device is lifted, insert the argon pipe into the tundish baking hole and the impact zone respectively, open the argon valve after placing it, and ensure that the argon replacement time is greater than 5min; adjust the position of the ladle car to ensure that each water outlet is centered; after the liquid level stabilizes, measure the insertion depth of the water nozzle to ensure that the insertion depth is between 180mm-220mm, and adjust it in time if it is not within the range.
[0048] After the ladle is poured, the long nozzle, tundish and immersion nozzle should be properly protected to ensure that the molten steel is isolated from the air, and the nozzle centering, nozzle insertion depth and tundish horizontal position should be properly controlled.
[0049] in,
[0050] When the molten steel in the tundish reaches 10t, the temperature measuring tube is vertically inserted into the molten steel to reduce the drift of the temperature measuring tube. The depth of the temperature measuring gun is >150mm.
[0051] After the pouring of the first ladle of the continuous casting tundish is completed, the contractor will promptly install the continuous temperature measurement thermocouple vertically on the tundish cover. After the second ladle is poured on the platform, manual temperature measurement is used for comparison with the continuous temperature measurement to ensure that the temperature difference is within ±2°C.
[0052] Normal pouring requires ensuring a high liquid level in the tundish. During the pouring process, the molten steel in the tundish must be poured at a high liquid level, and the liquid level depth of the tundish must be >850mm.
[0053] The pulling speed of the tail furnace of the tundish began to be reduced, and the pulling speed of the ∅450mm round billet was reduced from the original 0.55m / min to 0.45m / min, the F-EMS current was adjusted from 90A to 80A, and the specific water volume was adjusted from 0.095L / kg to 0.080L / kg; the pulling speed of the ∅500mm round billet was reduced from the original 0.45m / min to 0.35m / min; the pulling speed of the ∅600mm round billet was reduced from the original 0.33m / min to 0.23m / min; the pulling speed of the ∅700mm round billet was reduced from the original 0.24m / min to 0.18m / min; the pulling speed of the ∅800mm round billet was reduced from the original 0.19m / min to 0.15m / min.
[0054] The tail billet drawing time is extended, the length and width of the tail billet liquid phase hole are improved, the tail billet molten steel shrinkage is not good, and the water volume in the secondary cooling zone and the terminal electromagnetic stirring parameters are adjusted (F-EMS current is adjusted from 90A to 80A, and the specific water volume is adjusted from 0.095L / kg to 0.080L / kg) to reduce the stirring capacity. Due to the reduction in drawing speed, the billet grid will become thicker and the length of the liquid phase hole will become shorter. The stirring capacity needs to be reduced, otherwise a white bright band will appear (caused by too strong stirring capacity). At the same time, the specific water volume needs to be reduced to avoid excessive cooling and surface cracks.
[0055] For the shrinkage hole size standards for round billets, ∅500-13.4, ∅600 -15.65, ∅700-18.26, ∅800 20.87, those exceeding the standards are unqualified and need to be removed.
[0056] More specifically,
[0057] Jiangsu Shagang Group Huaigang Special Steel Co., Ltd. has carried out industrial production of 4130X-12, 30Mn2, S45Cr and other steel grades. The specific process is as follows:
[0058] Embodiment 1:
[0059] (1) During the 4130X-12 smelting in the LF process, after the alloy composition in the molten steel is adjusted to the target value in the middle of refining, the electrodes are energized to raise the temperature of the molten steel to liquidus + 70°C and the ladle is vacuum treated.
[0060] (2) The pulling speed of the last package of the continuous casting ∅600mm round billet was reduced from 0.33m / min to 0.23m / min. The F-EMS current was adjusted from 90A to 80A, and the F-EMS frequency was adjusted from 6HZ to 4HZ. The specific water content was adjusted from 0.095L / kg to 0.080L / kg.
[0061] (3) The superheat of the last furnace of the tundish is controlled between 23℃ and 27℃, the insulation effect of the tundish is good, the manual temperature measurement and continuous temperature measurement are within ±2℃, and the liquid level of the tundish is 854mm.
[0062] (4) The last ingot of each stream in the tail furnace was sawed and the cross section was inspected at low magnification. After analysis, the low magnification quality of the cross section of the ingot of 3.0m-4.0m was good, and no large shrinkage holes were found. However, the shrinkage holes at 2.5m from the tail were large and cracked, and the internal quality was poor.
[0063] The specific low-magnification quality ratings are shown in Table 1 and refer to Figure 1-8 .
[0064] Table 1 Data of shrinkage holes in each section
[0065]
[0066] Embodiment 2:
[0067] (1) During the 30Mn2 smelting in the LF process, after the alloy composition in the molten steel is adjusted to the target value in the middle of refining, the electrodes are energized to raise the temperature of the molten steel to liquidus + 80℃ and the ladle is vacuum treated.
[0068] (2) The pulling speed of the last package of the continuous casting round billet with a diameter of ∅800mm was reduced from 0.19m / min to 0.15m / min. The F-EMS current was adjusted from 240A to 220A, and the F-EMS frequency was adjusted from 4HZ to 3HZ. The specific water content was adjusted from 0.071L / kg to 0.066L / kg.
[0069] (3) The superheat of the last furnace of the tundish was controlled between 26℃ and 29℃, the insulation effect of the tundish was good, the manual temperature measurement and continuous temperature measurement were within ±2℃, and the liquid level of the tundish was 859mm.
[0070] (4) The last ingot of each stream in the tail furnace was sawed and the cross section was inspected at low magnification. After analysis, the low-magnification quality of the cross section of the 3.0m-4.0m ingot was good, and no large shrinkage holes were found. However, there was a long crack 2.5m away from the tail, and the internal quality was poor.
[0071] The specific low-magnification quality ratings are shown in Table 2 and refer to Figure 9-12 :
[0072] Table 2 Data of shrinkage holes in each section
[0073]
[0074] Embodiment 3:
[0075] (1) In the LF process of S45Cr smelting, after the alloy composition in the molten steel is adjusted to the target value in the middle of refining, the electrodes are energized to raise the temperature of the molten steel to liquidus + 80℃ and the ladle is vacuum treated.
[0076] (2) The pulling speed of the last package of the continuous casting ∅600mm round billet was reduced from 0.25m / min to 0.20m / min. The F-EMS current was adjusted from 270A to 250A, and the F-EMS frequency was adjusted from 5.5HZ to 4.5HZ. The specific water content was adjusted from 0.085L / kg to 0.078L / kg.
[0077] (3) The superheat of the last furnace of the tundish is controlled between 22℃-25℃, the insulation effect of the tundish is good, the manual temperature measurement and continuous temperature measurement are within ±2℃, and the liquid level of the tundish is 858mm.
[0078] (4) The last ingot of each stream in the tail furnace was sawed and the cross section was inspected at low magnification. After analysis, the low magnification quality of the cross section of the 3.0m-4.0m ingot was good, and no large shrinkage holes were found. However, the shrinkage holes at 2.5m from the tail were large and cracked, and the internal quality was poor.
[0079] The specific low-magnification quality ratings are shown in Table 3 and refer to Figure 13-20 .
[0080] Table 3 Data of shrinkage holes in each section.
[0081]
[0082] According to the test results of Examples 1-3, it can be concluded that the internal quality of 0m-2.5m scrapped billets is poor, and the shrinkage holes are densely distributed and large. To ensure product quality, cutting less than 2.5m should not be selected. To unify the operation, 3m is selected for tail billet cutting, and 3.5m can also be selected.
[0083] It should be noted that the above embodiments can be freely combined as needed. The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention, and these improvements and modifications should also be considered as the protection scope of the present invention.
Claims
1. A method for increasing the billet forming rate at the end of continuous casting of large-size round billets. It is characterized in that Reduce the pulling speed for the last package in the middle package; Adjust F-EMS current and specific water volume simultaneously; The tail billet cutting is divided into qualified billets and scrap billets. For 4130X-12 round billets with a diameter of 450-600mm, the pulling speed of the last package of the tundish was reduced from 0.33m / min to 0.23m / min, the F-EMS current was reduced from 90A to 80A, and the specific water content was adjusted from 0.095L / kg to 0.080L / kg. The tail billet is cut into scrap billets with a length of 3-3.5m, and the remaining finished billets are Continuous casting large-size round billet pouring process: In the middle of LF refining, after the alloy composition is adjusted to the target value, the temperature begins to rise to ensure the superheat of the continuous casting molten steel. After vacuum treatment, it is promptly sent to the continuous casting for pouring to ensure the smooth continuous casting pouring. In the process of power transmission and refining, add appropriate amount of slag surface deoxidation, control the white slag time ≥ 20 minutes, and do not add any materials 5 minutes before leaving the station. During the process of electrode power-on heating, the temperature of the first ladle rises to the liquidus temperature +70℃-90℃, and the temperature of the continuous casting furnace rises to the liquidus temperature +50℃-80℃; the continuous casting overheating degree is controlled at 15℃-35℃; for the molten steel that has passed the vacuum, the vacuum treatment station must ensure that the next ladle of the continuous casting furnace is hoisted to the continuous casting platform within 2 minutes before the molten steel of the previous continuous casting furnace is poured. After the ladle arrives at the platform, the ladle cover should be covered in time. After the ladle starts pouring, the temperature should be measured manually first, and the second ladle should be put into use for continuous temperature measurement. At the same time, each ladle needs to be calibrated manually to ensure the normal use of continuous temperature measurement and the accuracy of superheat. in, Before the ladle is poured, insert the argon blowing tube into the long water nozzle and adjust the flow rate to 40L / min; after the tundish baking device is lifted, insert the argon pipe into the tundish baking hole and the impact zone respectively, open the argon valve after placing it, and ensure that the argon replacement time is more than 5min; adjust the position of the ladle car to ensure that each water outlet is centered; after the liquid level is stable, measure the insertion depth of the water nozzle to ensure that the insertion depth is between 180mm-220mm. If it is not within the range, adjust it in time. After the ladle is poured, the long nozzle, tundish and immersion nozzle should be properly protected to ensure that the molten steel is isolated from the air, and the nozzle centering, nozzle insertion depth and tundish horizontal position should be properly controlled. in, When the molten steel in the tundish reaches 10t, the temperature measuring tube is vertically inserted into the molten steel to reduce the drift of the temperature measuring tube. The depth of the temperature measuring gun is >150mm. After the first ladle of continuous casting is poured, the contractor promptly places the continuous temperature measurement thermocouple vertically on the ladle cover. After the second ladle is poured, the manual temperature measurement is compared with the continuous temperature measurement to ensure that the temperature difference is within ±2°C. Normal pouring requires ensuring a high liquid level in the tundish. During the pouring process, the molten steel in the tundish must be poured at a high liquid level, and the liquid level depth of the tundish must be >850mm.
Citation Information
Patent Citations
Bearing steel continuous casting tail billet quality control method under unstable casting condition
CN109648055A
Method for reducing defects of tail section billet of high-alloy stainless steel billet
CN110877098A
Device and method for regulating and controlling flowing and solidification of secondary cooling area of special steel through dynamic combined magnetic fields
CN112974750A
Rapid sealing device and method for tail billet of oversized continuous casting round billet
CN115070001A
Method for preventing segregation and center porosity in continuous casting slab of steel
JP1996224650A