A slow-setting material for low-alkalinity cement-free refractory castable and preparation method thereof

By using the ordered hydrolysis mechanism of components such as alkaline lipase in low-alkalinity rho-alumina gel materials, suitable retarder materials are prepared, which solves the problem of the low hydrolysis rate of traditional retarder and the interference of acidic retarder. solve the problem, achieve efficient retardation and dispersion effects, and ensure the long-term stability of the material.

CN116332550BActive Publication Date: 2024-10-22WUHAN SANNDAR CHEM CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202310383135.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-04-12
Publication Date
2024-10-22
Estimated Expiration
2043-04-12

AI Technical Summary

Technical Problem

The hydrolysis rate of traditional esterification retarder in low-alkalinity ρ-alumina gel materials is low, making it difficult to achieve uniform retardation, and acidic retarder has a great impact on the initial setting time and fluidity, making it ineffective. Adjust the condensation speed of rho-alumina.

Method used

Using components such as alkaline lipase, glutaraldehyde, polymeric formaldehyde, oleic acid polyethylene glycol phosphate and polycarboxylate, the retardant material for low-alkalinity cement-free refractory castables is prepared through special synthesis and powdering processes. , utilizing the selective hydrolysis mechanism of alkaline lipase to perform orderly hydrolysis, control colloid formation, and enhance dispersion and anti-interference capabilities.

Benefits of technology

It achieves good retarding and dispersing effects on low-alkalinity ρ-alumina gel materials, improves the fluidity and stability of the material, and can be sealed and stored at room temperature for 24 months without failure.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004172953350000051
    Figure BDA0004172953350000051
Patent Text Reader

Abstract

The present invention provides a retarding material for low-alkalinity cement-free refractory castables, wherein the components and mass ratios of the retarding material are: 1 to 1.5 parts of alkaline lipase, 2 parts of glutaraldehyde, 100 parts of purified water, 20 to 40 parts of refined naphthalene, 20 to 40 parts of polymerized formaldehyde, 0.8 parts of concentrated sulfuric acid, 13 to 26 parts of oleic acid polyethylene glycol phosphate, and 3 to 15 parts of polycarboxylate. The retarding material adopts a special synthesis and powder making process, the powder is uniform, easy to use, and will not fail if sealed and stored for 24 months at room temperature. It has good retarding and dispersing effects on cement-free refractory castables with low-alkalinity ρ-alumina gel material as a binder, and has strong anti-interference ability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of refractory castables, and in particular to a retarding material for low-alkalinity cement-free refractory castables and a preparation method thereof. Background Art

[0002] Refractory castables mostly use calcium aluminate cement or pure calcium aluminate cement as a binder, such as high-alumina castables and corundum wear-resistant castables. However, cement-free refractory castables do not contain cement in their ingredients, but instead add micropowder or sol to produce agglomeration and bonding. Cement-free refractory castables are composed of refractory aggregates, powders, binders and admixtures. Generally, oxides with the same chemical composition as the main material of the castable, or synthetic compound ultrafine powders, or oxide sols are used as binders. This binder has a low impurity content, so it does not reduce the refractoriness and resistance to slag erosion of the castable, and can produce self-bonding during use, which helps to improve the strength of high-temperature structures.

[0003] ρ-alumina has the advantages of high temperature resistance, corrosion resistance and good volume stability. It can be used as a binder for cement-free refractory castables and is widely used in corundum, high-alumina, and aluminum-magnesium refractory castables. However, in refractory castables with ρ-alumina low-alkalinity gel material as a binder, the setting speed is relatively fast, and retarding materials are usually required to be added for adjustment. However, due to the low alkalinity of ρ-alumina, the hydrolysis rate of traditional esterified retarders is low, and it is difficult to achieve a more uniform retarding effect. At the same time, traditional acidic retarders have a greater interference in the early stage of colloid formation of refractory castables with low alkalinity, thereby having a greater impact on the fluidity and initial setting time of the castable. Therefore, it is necessary to develop a new retarding material that can be applied to ρ-alumina low-alkalinity cement-free refractory castables. Summary of the invention

[0004] In view of the above-mentioned deficiencies in the prior art, the present invention provides a retarding material for low-alkalinity cement-free refractory castables. The retarding material adopts a special synthesis and powder making process, the powder is uniform, and it is easy and convenient to use. It will not become invalid if it is sealed and stored for 24 months at room temperature. It has good retarding and dispersing effects on cement-free refractory castables with low-alkalinity ρ-alumina gel material as a binder, and has strong anti-interference ability.

[0005] The technical solution adopted to achieve the above-mentioned purpose of the present invention is:

[0006] The invention discloses a retarding material for low-alkalinity cement-free refractory castables. The components and mass proportions of the retarding material are as follows: 1-1.5 parts of alkaline lipase, 2-4 parts of glutaraldehyde, 90-100 parts of purified water, 20-40 parts of refined naphthalene, 20-40 parts of polymerized formaldehyde, 0.6-0.8 parts of concentrated sulfuric acid, 13-26 parts of oleic acid polyethylene glycol phosphate, and 3-15 parts of polycarboxylate.

[0007] The alkaline lipase has a tolerable pH range of 4 to 10, a tolerable temperature range of 10 to 50° C., and an enzyme activity higher than 50,000 u / g.

[0008] The glutaraldehyde is a 35-40% glutaraldehyde solution.

[0009] The molecular weight of polyethylene glycol in the synthetic raw material of the oleic acid polyethylene glycol phosphate is 100-3000.

[0010] The polycarboxylate is any polycarboxylate with a molecular weight between 10,000 and 30,000 and a pH value between 6.5 and 7.5, which is copolymerized by monovinyl polyoxyethylene ester and maleic acid in an acid ester ratio of 1:2 to 1:6, wherein the molecular weight of the monovinyl polyoxyethylene ester is 1,400 to 1,600.

[0011] The refined naphthalene is high-purity refined naphthalene with a sulfur content lower than 0.05%.

[0012] The polymerized formaldehyde is prepared by mixing dioxymethylene and trioxymethylene in a mass ratio of 2:1 to 4:1, and the content of dioxymethylene and trioxymethylene is higher than 98%.

[0013] The concentrated sulfuric acid is a sulfuric acid solution with a mass fraction greater than 70%.

[0014] The purified water is secondary purified water that meets the requirements of the Chinese Pharmacopoeia.

[0015] The present invention also provides a method for preparing a slow-setting material for low-alkalinity cement-free refractory castables, comprising the following steps: (1) placing concentrated sulfuric acid and refined naphthalene in a medium-pressure reactor, heating the mixture to 80-85°C, and stirring the mixture for 30-40 minutes. After the mixture is free of leakage and abnormality, slowly heating the mixture to 155-160°C and reacting the mixture for 1-1.5 hours. (2) after the reaction is completed, placing the mixture in a normal-pressure reactor, adding polymerized formaldehyde and purified water, and performing a cross-linking reaction at 75-80°C for 3-3.5 hours. After the reaction is completed, cooling the mixture to below 40°C, adjusting the pH value to between 7 and 7.5 with an alkali solution, and allowing the mixture to stand for 1-1.5 hours. (3) adding alkaline lipase and glutaraldehyde, and stirring the mixture for 40-45 minutes while maintaining the temperature at 30-35°C. (4) spraying the mixture into powder using a spray dryer at an inlet temperature of 120°C, and uniformly mixing the powder with oleic acid polyethylene glycol phosphate and polycarboxylic acid ester to obtain a slow-setting material for low-alkalinity cement-free refractory castables.

[0016] Compared with the prior art, the retarding material for low-alkalinity cement-free refractory castables provided by the present invention has the following advantages: 1. In the present invention, a short-chain compound synthesized by concentrated sulfuric acid, refined naphthalene, polymerized formaldehyde and purified water is used as a template, and alkaline lipase is fixed on the template by pentanediol. The selective hydrolysis mechanism of alkaline lipase is utilized to orderly and gradually hydrolyze oleic acid polyethylene glycol phosphate and polycarboxylic acid ester, and the hydrolysis process responds to the pH value, and the gradual hydrolysis after the formation of the colloid can be controlled without affecting the fluidity in the early stage. It is suitable for cement-free refractory castables with low-alkalinity ρ-alumina gel material as a binder, has good retarding and dispersing effects, and has strong anti-interference ability; at the same time, since oleic acid polyethylene glycol phosphate, polycarboxylic acid ester and sulfonated condensates generated by polymerized formaldehyde and refined naphthalene are all surface-active structures, the fluidity of the overall material is improved, and the dispersing effect is further improved.

[0017] 2. The present invention adopts a special synthesis and powder making process, and the obtained retarding material for low-alkalinity cement-free refractory castable is in powder state, the average particle size of the particles is between 12μm and 25μm, the powder is uniform, easy to use, and will not become invalid if sealed and stored for 24 months at room temperature. DETAILED DESCRIPTION

[0018] In order to enable those skilled in the art to better understand the technical solution of the present invention, the present invention is further described in detail below in conjunction with embodiments.

[0019] In the following examples, the alkaline lipase has a tolerance pH range of 4 to 10, a tolerance temperature of 10 to 50° C., and an enzyme activity of more than 50,000 u / g. Glutaraldehyde is a 35 to 40% glutaraldehyde solution. The molecular weight of polyethylene glycol in the synthetic raw material of oleic acid polyethylene glycol phosphate is 100 to 3,000. Polycarboxylate is a copolymer of monovinyl polyoxyethylene ester and maleic acid according to an acid ester ratio of 1:2 to 1:6, with a molecular weight between 10,000 and 30,000 and a pH value of 6.5 to 7.5, wherein the molecular weight of monovinyl polyoxyethylene ester is 1,400 to 1,600. Refined naphthalene is a high-purity refined naphthalene with a sulfur content of less than 0.05%. Polyformaldehyde is a mixture of dioxane and trioxane in a mass ratio of 2:1 to 4:1, and the content of dioxane and trioxane is higher than 98%. Concentrated sulfuric acid is a sulfuric acid solution with a mass fraction greater than 70%. Purified water is secondary purified water that meets the requirements of the Chinese Pharmacopoeia.

[0020] Example 1

[0021] The components and mass ratios of the retarding material for low-alkalinity cement-free refractory castable provided in this embodiment are: 1 part of alkaline lipase, 2 parts of glutaraldehyde, 100 parts of purified water, 40 parts of refined naphthalene, 20 parts of polymerized formaldehyde, 0.8 parts of concentrated sulfuric acid, 26 parts of oleic acid polyethylene glycol phosphate, and 3 parts of polycarboxylate.

[0022] The preparation method comprises the following steps: (1) placing concentrated sulfuric acid and refined naphthalene in a medium-pressure reactor, heating the mixture to 80°C, and stirring the mixture for 30 minutes. After no leakage or abnormality is observed, the mixture is slowly heated to 160°C for reaction for 1.5 hours. (2) after the reaction is completed, the mixture is placed in a normal-pressure reactor, and polymerized formaldehyde and purified water are added thereto. The mixture is subjected to a cross-linking reaction at 80°C for 3 hours. After the reaction is completed, the mixture is cooled to below 40°C, and the pH value is adjusted to between 7 and 7.5 with an alkali solution, and the mixture is allowed to stand for 1 hour. (3) alkaline lipase and glutaraldehyde are added thereto, and the mixture is stirred for 40 minutes while the temperature is maintained at 30 to 35°C. (4) the mixture is sprayed into powder at an inlet temperature of 120°C using a spray dryer. After the powder is formed, the mixture is uniformly mixed with oleic acid polyethylene glycol phosphate and polycarboxylic acid ester to obtain a slow-setting material for low-alkalinity cement-free refractory castables.

[0023] Example 2

[0024] The preparation method of Example 2 is basically the same as that of Example 1, and the only difference is the formula of the retarding material for low-alkalinity cement-free refractory castable. The components and mass ratios of the retarding material for low-alkalinity cement-free refractory castable provided in Example 2 are: 1 part of alkaline lipase, 2 parts of glutaraldehyde, 100 parts of purified water, 20 parts of refined naphthalene, 30 parts of polymerized formaldehyde, 0.8 parts of concentrated sulfuric acid, 13 parts of oleic acid polyethylene glycol phosphate, and 15 parts of polycarboxylate.

[0025] Example 3

[0026] The preparation method of Example 3 is basically the same as that of Example 1, and the only difference is that the formula of the retarding material for low-alkalinity cement-free refractory castable is different. The components and mass ratio of the retarding material for low-alkalinity cement-free refractory castable provided in Example 3 are: 1.2 parts of alkaline lipase, 2 parts of glutaraldehyde, 100 parts of purified water, 30 parts of refined naphthalene, 30 parts of polymerized formaldehyde, 0.8 parts of concentrated sulfuric acid, 20 parts of oleic acid polyethylene glycol phosphate, and 10 parts of polycarboxylate.

[0027] Example 4

[0028] The preparation method of Example 4 is basically the same as that of Example 1, and the only difference is that the formula of the retarding material for low-alkalinity cement-free refractory castable is different. The components and mass ratio of the retarding material for low-alkalinity cement-free refractory castable provided in Example 4 are: 1.5 parts of alkaline lipase, 2 parts of glutaraldehyde, 100 parts of purified water, 20 parts of refined naphthalene, 40 parts of polymerized formaldehyde, 0.8 parts of concentrated sulfuric acid, 15 parts of oleic acid polyethylene glycol phosphate, and 8 parts of polycarboxylate.

[0029] Example 5

[0030] The preparation method of Example 5 is basically the same as that of Example 1, and the only difference is that the formula of the retarding material for low-alkalinity cement-free refractory castable is different. The components and mass ratio of the retarding material for low-alkalinity cement-free refractory castable provided in Example 5 are: 1.4 parts of alkaline lipase, 2 parts of glutaraldehyde, 100 parts of purified water, 40 parts of refined naphthalene, 40 parts of polymerized formaldehyde, 0.8 parts of concentrated sulfuric acid, 18 parts of oleic acid polyethylene glycol phosphate, and 12 parts of polycarboxylate.

[0031] The product properties of the slow-setting materials for low-alkalinity cement-free refractory castables obtained in Examples 1 to 5 were tested, and the results are shown in the following table.

[0032] The density is tested according to GB / T 31057.2-2018, the dissolved residue is tested according to GB / T 9738-2008, the ignition residue is tested according to GB / T 7531-2008, and the average particle size is tested according to GB / T 29022-2021.

[0033] project Example 1 Example 2 Example 3 Example 4 Example 5 Appearance powder powder powder powder powder Density(g / mL) 1.03 1.05 1.1 1.02 1.04 1% aqueous solution pH 6.35 6.14 6.5 6.2 63 Dissolved residue 3% 3% 3% 3% 3% Burning residue 8% 8% 8% 8% 8% Average particle size (μm) 15 16 20 18 19

[0034] The retarding materials for low-alkalinity cement-free refractory castables obtained in Examples 1 to 5 were sealed and stored for 24 months at room temperature, and the product performance was tested again, and there was no obvious difference in the product performance, indicating that the retarding materials provided by the present invention will not fail when sealed and stored for 24 months at room temperature, and have good stability.

[0035] Application Examples

[0036] The retarding materials for low-alkalinity cement-free refractory castables obtained in Examples 1 to 5, as well as the esterified retarder and the acidic retarder purchased from the market were added to the ρ-alumina slurry (for the sake of data simplification, only the pure slurry experiment was performed in the application example, and there was only ρ-alumina in the slurry), and the added amount was 0.1% (mass fraction). The setting properties of the ρ-alumina slurry were tested, and the results are shown in the following table.

[0037] The dispersion force is tested according to GBT 5550-2016 Determination of dispersion force of surfactants (standard status: current) standard, and the water seepage performance is tested according to GB / T 22459.8-2021 standard.

[0038]

[0039] It can be seen from the above table that the retarding materials obtained in Examples 1 to 5 have obvious viscosity reducing and retarding effects when used in ρ-alumina slurry, and can also provide a certain degree of anti-settling property.

Claims

1. A slow-setting material for low-alkalinity cement-free refractory castables, characterized in that: The components and mass proportions of the retarding material are: 1-1.5 parts of alkaline lipase, 2-4 parts of glutaraldehyde, 90-100 parts of purified water, 20-40 parts of refined naphthalene, 20-40 parts of polymerized formaldehyde, 0.6-0.8 parts of concentrated sulfuric acid, 13-26 parts of oleic acid polyethylene glycol phosphate, and 3-15 parts of polycarboxylate; the polycarboxylate is any polycarboxylate with a molecular weight between 10000 and 30000 and a pH value between 6.5 and 7.5, which is copolymerized with monovinyl polyoxyethylene ester and maleic acid in a ester ratio of 1:2-1:6, wherein the molecular weight of monovinyl polyoxyethylene ester is 1400-1600; the polymerized formaldehyde is a mixture of dioxymethylene and trioxymethylene in a mass ratio of 2:1-4:

1.

2. The slow-setting material for low-alkalinity cement-free refractory castable according to claim 1, characterized in that: The alkaline lipase has a tolerable pH range of 4-10, a tolerable temperature of 10-50° C., and an enzyme activity higher than 50000 u / g.

3. The slow-setting material for low-alkalinity cement-free refractory castable according to claim 1, characterized in that: The glutaraldehyde is a 35% to 40% glutaraldehyde solution.

4. The slow-setting material for low-alkalinity cement-free refractory castable according to claim 1, characterized in that: The molecular weight of polyethylene glycol in the synthetic raw material of the oleic acid polyethylene glycol phosphate is 100-3000.

5. The slow-setting material for low-alkalinity cement-free refractory castable according to claim 1, characterized in that: The refined naphthalene is high-purity refined naphthalene with a sulfur content of less than 0.05%.

6. The slow-setting material for low-alkalinity cement-free refractory castable according to claim 1, characterized in that: The content of trioxymethylene and trioxymethylene in the polymerized formaldehyde is higher than 98%.

7. The slow-setting material for low-alkalinity cement-free refractory castable according to claim 1, characterized in that: The concentrated sulfuric acid is a sulfuric acid solution with a mass fraction greater than 70%.

8. The slow-setting material for low-alkalinity cement-free refractory castable according to claim 1, characterized in that: The purified water is secondary purified water that meets the requirements of the Chinese Pharmacopoeia.

9. A method for preparing a slow-setting material for low-alkalinity cement-free refractory castables according to claim 1, characterized in that The following steps are involved: (1) Concentrated sulfuric acid and refined naphthalene are placed in a medium-pressure reactor, and the temperature is raised to 80-85°C. The mixture is stirred for 30-40 minutes at this temperature. After no leakage or abnormality is found, the temperature is slowly raised to 155-160°C for reaction for 1-1.5 hours. (2) After the reaction is completed, the mixture is placed in a normal-pressure reactor and polymerized formaldehyde and purified water are added. The mixture is subjected to a cross-linking reaction at 75-80°C for 3-3.5 hours. After the reaction is completed, the mixture is cooled to below 40°C, and the pH value is adjusted to between 7 and 7.5 with an alkali solution. The mixture is allowed to stand for 1-1.5 hours. (3) Alkaline lipase and glutaraldehyde are added thereto, and the mixture is stirred for 40-45 minutes at a temperature maintained at 30-35°C. (4) The mixture is sprayed into powder using a spray dryer at an inlet temperature of 120°C. The powder is then mixed evenly with oleic acid polyethylene glycol phosphate and polycarboxylic acid ester to obtain a slow-setting material for low-alkalinity cement-free refractory castables.

Citation Information

Patent Citations

  • Retarders for hardening phenolic resins

    CA2046060A1

  • Impurity-resistant water reducing agent for high-silica-fume refractory castable and preparation method of impurity-resistant water reducing agent

    CN113563556A

  • MULTICOMPONENT CONCRETE SUPERPLASTICIZER

    SE8206104D0

  • Use of water-soluble mixed polymers as a flowing medium and / or as a hardening retarder for refractory materials which contain aluminate cement

    US6995105B1