A metamaterial and its preparation method

By using dihydrogen phosphate complexes to prepare metamaterials, the problems of poor stability and high-temperature resistance of existing metamaterials have been solved, and the high-temperature stability and electromagnetic properties have been improved, reducing production costs and broadening the application range.

CN116345167BActive Publication Date: 2026-11-10DONGGUAN KEFU PRECISION MFG CO LTD +2
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202111602557.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-12-24
Publication Date
2026-11-10
Estimated Expiration
2041-12-24

AI Technical Summary

Technical Problem

Existing metamaterials suffer from poor stability and high-temperature resistance, and their processing is complex and costly, which limits their application scope.

Method used

Metamaterials with superior electromagnetic and self-adhesive properties were prepared by using dihydrogen phosphate complexes as microstructure materials, forming multilayer microstructures on a substrate, and sintering them at a specific temperature.

Benefits of technology

It achieves high-temperature and chemical stability of metamaterials, reduces production costs, broadens the application range, and possesses good electromagnetic response characteristics and self-adhesive properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116345167B_ABST
    Figure CN116345167B_ABST
Patent Text Reader

Abstract

This invention relates to a metamaterial and its preparation method. The material comprises at least one substrate and at least one microstructure layer. The at least one microstructure layer is disposed on the at least one substrate. The microstructure layer comprises multiple microstructures, and the material of the multiple microstructures includes a dihydrogen phosphate complex, wherein the dihydrogen phosphate complex comprises dihydrogen phosphate and titanate or barium lanthanum titanium. The metamaterial of one embodiment of this invention, compared with existing metallic artificial microstructure metamaterials, not only possesses superior electromagnetic and self-adhesive properties, but also exhibits good high-temperature stability and chemical stability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to artificial electromagnetic materials, and more particularly to a metamaterial with high temperature resistance and good electromagnetic and adhesive properties. Background Technology

[0002] Metamaterials refer to artificial composite structures or materials that possess extraordinary physical properties not found in natural materials. Through precise design of the material's geometry, it is possible to overcome certain apparent natural laws, thereby obtaining extraordinary material functions that surpass the inherent properties of materials found in nature. The functionality of metamaterials is primarily achieved by designing different structures and shapes for artificial microstructures, which can alter the electromagnetic response characteristics of the metamaterials.

[0003] Artificial microstructures typically refer to planar or three-dimensional metallic microstructures composed of geometrically arranged patterns according to a specific rule. Existing metallic microstructure fabrication methods generally involve first forming a metal film using processes such as thermal evaporation, sputtering, chemical deposition, or electron beam deposition, followed by fabrication using methods like laser etching, plasma etching, or chemical etching to create the microstructure pattern. This method of fabrication is complex, requires expensive equipment, and has a long processing cycle. Metallic microstructures also exhibit poor stability, being prone to detachment, oxidation, and high-temperature resistance, significantly reducing their environmental adaptability and application range. Furthermore, although noble metal microstructures can withstand high temperatures, the high price of precious metals greatly increases production costs, hindering industrialization. Therefore, developing novel metamaterials with equivalent metallic microstructure metamaterials is essential. Summary of the Invention

[0004] Based on the above analysis, one embodiment of the present invention aims to provide a metamaterial to solve the problems of poor stability and poor high-temperature resistance of existing metamaterials.

[0005] On one hand, one embodiment of the present invention provides a metamaterial, comprising:

[0006] At least one substrate; and

[0007] At least one microstructure layer is disposed on the at least one substrate;

[0008] The at least one microstructure layer comprises multiple microstructures, and the material of the multiple microstructures includes a dihydrogen phosphate complex, wherein the dihydrogen phosphate complex comprises dihydrogen phosphate and titanate or barium lanthanum titanium.

[0009] According to one embodiment of the present invention, the dihydrogen phosphate salt includes one or more of aluminum dihydrogen phosphate, magnesium dihydrogen phosphate, sodium dihydrogen phosphate, and disodium hydrogen phosphate; and / or,

[0010] The titanate includes one or more of strontium titanate, barium titanate, calcium titanate, and magnesium titanate.

[0011] According to one embodiment of the present invention, the mass ratio of the dihydrogen phosphate to the titanate or the barium lanthanum titanium is 1:1 to 1:3; and / or,

[0012] The dielectric constant of the titanate or the barium lanthanum titanium is 30 to 500.

[0013] According to one embodiment of the present invention, the at least one substrate includes a first substrate, the first substrate including a first surface and a second surface disposed opposite to the first surface; the at least one microstructure layer includes a first microstructure layer and a second microstructure layer; the first microstructure layer is disposed on the first surface and includes one or more first microstructures; the second microstructure layer is disposed on the second surface and includes one or more second microstructures; one or more first through-holes are provided in the metamaterial, each first through-hole penetrating one first microstructure, the first substrate and a second microstructure.

[0014] According to one embodiment of the present invention, the at least one substrate further includes a second substrate, and the at least one microstructure layer further includes a third microstructure layer; the third microstructure layer includes one or more third microstructures; the second substrate includes a third surface and a fourth surface disposed opposite to the third surface, the third surface is disposed on the second surface of the first substrate, and the second microstructure layer is sandwiched between the second surface and the third surface; the third microstructure layer is disposed on the fourth surface, and one or more second through holes are formed on the second substrate and the third microstructure layer, each second through hole penetrating the second substrate and one of the third microstructures, and each second through hole communicating with a first through hole.

[0015] According to one embodiment of the present invention, the plurality of microstructures include one or more of the following: herringbone structure, I-shaped structure, square structure, cross-shaped structure, L-shaped structure, Y-shaped structure, spiral structure, circular structure, square structure, column-rectangular structure, elliptical structure, and rhombus structure.

[0016] According to one embodiment of the present invention, a groove is formed on each of the first microstructure, each of the second microstructure and each of the third microstructure.

[0017] According to one embodiment of the present invention, a first groove is formed on each of the first microstructures, a second groove is formed on each of the second microstructures, and a third groove is formed on each of the third microstructures; and / or,

[0018] The angle between the axis of the first through hole, the axis of the second through hole and the first surface and / or the second surface is 85° to 95°.

[0019] An embodiment of the present invention further provides a method for preparing the above-mentioned metamaterial, comprising:

[0020] A dihydrogen phosphate complex is provided, the dihydrogen phosphate complex comprising a dihydrogen phosphate, a titanate or barium lanthanum titanium, and a solvent;

[0021] Using the aforementioned dihydrogen phosphate complex as a raw material, a plurality of pre-formed microstructures are formed on at least one substrate to obtain a pre-formed metamaterial; and

[0022] The preformed metamaterial is sintered to obtain the metamaterial.

[0023] According to one embodiment of the present invention, the preparation method includes drying the preformed metamaterial at a stepped temperature, wherein the drying at the stepped temperature includes: holding at 80-90°C for 4-6 hours, holding at 90-100°C for 3-5 hours, and holding at 100-200°C for 2-3 hours.

[0024] According to one embodiment of the present invention, the preparation method includes subjecting the pre-formed metamaterial after drying to a stepped high-temperature sintering treatment, wherein the stepped high-temperature treatment includes:

[0025] The temperature is increased from 20-30℃ to 300-500℃ at a heating rate of 2-5℃ / min and held for 4-6 hours. Then the temperature is increased from 300-500℃ to 500-800℃ at a heating rate of 5-8℃ / min and held for 3-5 hours. Finally, the temperature is increased from 500-800℃ to 800-1000℃ at a heating rate of 10-15℃ / min and held for 2-3 hours.

[0026] The metamaterial of one embodiment of the present invention, compared with existing metal microstructure metamaterials, not only has superior electromagnetic properties and self-adhesive properties, but also has good high-temperature stability and chemical stability.

[0027] In this invention, the above-described technical solutions can be combined with each other to achieve more preferred combinations. Other features and advantages of this invention will be set forth in the following description, and some advantages may become apparent from the description or be learned by practicing the invention. The objects and other advantages of this invention can be realized and obtained from what is particularly pointed out in the description and drawings. Attached Figure Description

[0028] The accompanying drawings are for illustrative purposes only and are not intended to limit the scope of the invention. Wherein:

[0029] Figure 1This is a top view of a metamaterial with a three-layer microstructure according to an embodiment of the present invention;

[0030] Figure 2 This is a cross-sectional view of a metamaterial with a three-layer microstructure according to an embodiment of the present invention;

[0031] Figure 3 for Figure 2 Enlarged schematic diagrams of individual first, second, and third microstructures;

[0032] Figure 4 for Figure 3 Top view of the structure

[0033] Figure 5 This is a top view of the metamaterial of Embodiment 1 of the present invention;

[0034] Figure 6 This is a top view of the metamaterial of Embodiment 2 of the present invention;

[0035] Figure 7 for Figure 6 A magnified view of a microstructure in the image;

[0036] Figure 8 This is a top view of the metamaterial of Embodiment 3 of the present invention;

[0037] Figure 9 for Figure 8 Enlarged view of the microstructure of the middle part;

[0038] Figures 10a to 10i These are the transmittance test diagrams of the metamaterials in Example 1 and Comparative Example 1 of the present invention;

[0039] Figure 11 The figures show the insertion loss and return loss test results of the metamaterial in Embodiment 2 of the present invention.

[0040] Figure 12 This is a test diagram of the beam pattern of the metamaterial in Embodiment 3 of the present invention.

[0041] Figure 13a The transmittance test diagram is shown for electromagnetic waves incident on the metamaterials of Embodiment 4 and Comparative Example 2 of the present invention.

[0042] Figure 13b The image shows the transmittance test results of electromagnetic waves incident on the metamaterials of Embodiment 4 and Comparative Example 3 of this invention. Detailed Implementation

[0043] The preferred embodiments of the present invention will be described in detail below. The accompanying drawings constitute a part of the present invention and are used together with the embodiments of the present invention to illustrate the principles of the present invention, but are not intended to limit the scope of the present invention.

[0044] One embodiment of the present invention provides a metamaterial, comprising:

[0045] At least one substrate; and

[0046] At least one microstructure layer is disposed on the substrate;

[0047] Among them, at least one microstructure layer includes multiple microstructures, and the material of the microstructures includes a dihydrogen phosphate complex, which includes dihydrogen phosphate and titanate or barium lanthanum titanium.

[0048] The metamaterial of one embodiment of the present invention uses dihydrogen phosphate material as a self-adhesive, which can form a strong bond with the substrate under high temperature, and the dihydrogen phosphate composite can work stably for a long time above 1000°C. Therefore, excellent electromagnetic properties can be achieved through appropriate structural design and arrangement.

[0049] In one embodiment, the dihydrogen phosphate complex includes dihydrogen phosphate and titanate.

[0050] In another embodiment, the dihydrogen phosphate complex comprises dihydrogen phosphate and barium lanthanum titanium.

[0051] In one embodiment, the dihydrogen phosphate salt may be one or more of aluminum dihydrogen phosphate, magnesium dihydrogen phosphate, sodium dihydrogen phosphate, and disodium hydrogen phosphate.

[0052] In one embodiment, the titanate may be one or more of strontium titanate, barium titanate, barium strontium titanate, calcium titanate, and magnesium titanate.

[0053] In one embodiment, the titanate is barium strontium titanate, which includes strontium titanate and barium titanate.

[0054] In one embodiment, the dielectric constant of the titanate or barium lanthanum titanium is 30 to 500, for example 50, 80, 100, 150, 200, 250, 300, 350, 400, 450.

[0055] In one embodiment, the mass ratio of dihydrogen phosphate to titanate (or barium lanthanum titanium) is dihydrogen phosphate: titanate (or barium lanthanum titanium) = 1:1 to 1:3, for example 1:1.2, 1:1.5, 1:1.8, 1:2, 1:2.2, 1:2.5, 1:2.8.

[0056] In one embodiment, the microstructure may be disposed on one surface of the substrate or on two opposite surfaces of the substrate.

[0057] Reference Figures 1 to 4As shown, in one embodiment, at least one substrate includes a first substrate 10 and a second substrate 20. The first substrate 10 includes a first surface 11 and a second surface disposed opposite to the first surface 11. The second substrate 20 includes a third surface and a fourth surface 21 disposed opposite to the third surface. A first microstructure layer is disposed on the first surface 11, and the first microstructure layer includes one or more first microstructures 31. A second microstructure layer is disposed on the second surface, and the second microstructure layer includes one or more second microstructures 32. A third microstructure layer is disposed on the fourth surface 21, and the third microstructure layer includes one or more second microstructures 32. The third microstructure 33; one or more first through holes 41 are provided in the metamaterial, each first through hole 41 penetrating a first microstructure 31, a first substrate 10 and a second microstructure 32; one or more second through holes 42 are formed on the second substrate 20 and the third microstructure layer, each second through hole 42 penetrating the second substrate 20 and a third microstructure 33, and each second through hole 42 is connected to a first through hole 41, that is, the first through hole 41 and the second through hole 42 penetrate the first microstructure 31, the first substrate 10, the second microstructure 32, the second substrate 20 and the third microstructure 33.

[0058] In one embodiment, the plurality of first microstructures 31, the plurality of second microstructures 32 and the plurality of second microstructures 33 are arranged in an array, such as a square array. Further, the square array can be a 5×5 array, an 8×8 array, etc.

[0059] In one embodiment, a plurality of first microstructures 31 are arranged in a square array, and the distance between the center points of two adjacent first microstructures 31 is L1; a plurality of second microstructures 32 are arranged in a square array, and the distance between the center points of two adjacent second microstructures 32 is L2; ​​a plurality of third microstructures 33 are arranged in a square array, and the distance between the center points of two adjacent third microstructures 33 is L3; preferably, L1 equals L2 equals L3.

[0060] In one embodiment, the number of first microstructures 31, second microstructures 32, and third microstructures 33 is the same. Each first microstructure 31 is disposed opposite to one second microstructure 32 and one third microstructure. That is, along the direction perpendicular to the first surface 11, the second surface, and the fourth surface 21 (i.e., the thickness direction of the first substrate 10), the projection of the first microstructure 31 and at least part of the projection of the second microstructure 32 and the third microstructure 33 overlap. Further, the projection of the first microstructure 31 and the projection of the second microstructure 32 and the third microstructure 33 completely overlap.

[0061] In one embodiment, along the thickness direction of the first substrate 10 and the second substrate 20, the projections of the first microstructure layer, the second microstructure layer, and the third microstructure layer completely overlap.

[0062] In one embodiment, the first microstructure 31, the second microstructure 32, and the third microstructure 33 are the same. For example, the first microstructure 31 and / or the second microstructure 32 and / or the third microstructure 33 can be a herringbone structure, an I-shaped structure, a square structure, a cross-shaped structure, an L-shaped structure, a Y-shaped structure, a loop-shaped structure, a circular structure, a square structure, a column-rectangular structure, an elliptical structure, or a rhombus structure.

[0063] In one embodiment, the first microstructure 31 and / or the second microstructure 32 and / or the third microstructure 33 are square structures with a side length of 2.5 to 3.5 mm, or more specifically 3.25 to 3.45 mm, such as 2.7 mm, 2.8 mm, 2.9 mm, 3.0 mm, 3.1 mm, 3.2 mm, 3.3 mm, or 3.4 mm; and a thickness of 0.03 to 0.04 mm, such as 0.035 mm.

[0064] In one embodiment, the first surface 11, the second surface, and the fourth surface 21 are parallel to each other along the thickness direction of the first substrate 10 and the second substrate 20. Each first microstructure 31 is disposed opposite to a second microstructure 32 and a third microstructure 33. A first through hole 41 passes through the first microstructure 31, the second microstructure 32, and the first substrate 10 sandwiched between them. Each second through hole 42 is connected to a first through hole 41, that is, the first through hole 41 and the second through hole 42 pass through the first microstructure 31, the first substrate 10, the second microstructure 32, the second substrate 20, and the third microstructure 33.

[0065] In one embodiment, the angle between the axis of the first through hole 41 and the first surface 11 and / or the second surface is 85 to 95°, for example, the axis of the first through hole 41 is perpendicular to the first surface 11 and / or the second surface; the angle between the axis of the second through hole 42 and the second surface and / or the fourth surface 21 is 85 to 95°, for example, the axis of the second through hole 42 is perpendicular to the second surface and / or the fourth surface 21.

[0066] In one embodiment, the first through hole 41 and the second through hole 42 can be circular holes, and the radius of the cross-section (the cross-section perpendicular to the axial direction) of the circular hole can be 0.1 to 0.3 mm, for example 0.15 mm, 0.20 mm, or 0.25 mm.

[0067] In one embodiment, the first through hole 41 and the second through hole 42 have the same axis; the first through hole 41 and the second through hole 42 are through holes with the same cross-sectional radius and depth; the number of the first through hole 41 and the second through hole 42 is the same as the number of the first microstructure 31, the second microstructure 32, and the third microstructure 33.

[0068] In one embodiment, a first microstructure 31 and a second microstructure 32 are respectively provided at both ends of each first through hole 41. The first microstructure 31 and the second microstructure 32 are both made of dihydrogen phosphate complex. A dihydrogen phosphate complex layer is provided on the hole wall of the first through hole 41. Further, the dihydrogen phosphate complex layer on the hole wall of the first through hole 41 is connected to the first microstructure 31 and the second microstructure 32 respectively. A second microstructure 32 and a third microstructure 33 are respectively provided at both ends of each second through hole 42. The second microstructure 32 and the third microstructure 33 are both made of dihydrogen phosphate. A dihydrogen phosphate layer is provided on the hole wall of the second through hole 42. Further, the dihydrogen phosphate layer on the hole wall of the second through hole 42 is connected to the second microstructure 32 and the third microstructure 33 respectively.

[0069] In one embodiment, grooves are provided on the first microstructure 31, the second microstructure 32, and the third microstructure 33. The grooves can increase the bandwidth and application range of the metamaterial.

[0070] In one embodiment, reference is made to Figures 1 to 4 As shown, a first groove 51 is formed on each first microstructure 31, and the first groove 51 penetrates the first microstructure 31 along the thickness direction of the first microstructure 31, that is, the depth of the first groove 51 is the same as the thickness of the first microstructure 31; similarly, a second groove 52 is formed on each second microstructure 32, and the second groove 52 penetrates the second microstructure 32 along the thickness direction of the second microstructure 32; a third groove 53 is formed on each third microstructure 33, and the third groove 53 penetrates the third microstructure 33 along the thickness direction of the third microstructure 33.

[0071] In one embodiment, the lengths of the first groove 51, the second groove 52, and the third groove 53 can be 2.7 to 4.3 mm, such as 3.0 mm, 3.2 mm, 3.5 mm, 3.8 mm, 4.0 mm, 4.2 mm, etc.

[0072] In one embodiment, the width W of the first groove 51, the second groove 52, and the third groove 53 can be 0.06 to 0.14 mm, for example, 0.08 mm, 0.1 mm, 0.12 mm, etc.

[0073] In one embodiment, the first groove 51, the second groove 52, and the third groove 53 are not annular structures, that is, one end of the groove is not connected to the other end along the length direction of the groove.

[0074] In one embodiment, the first groove 51, the second groove 52, and the third groove 53 are U-shaped or U-shaped; further, the angle between the U-shaped or U-shaped opening direction of the first groove 51 and the U-shaped or U-shaped opening direction of the second groove 52 is greater than 0° and less than or equal to 90°, and the angle between the U-shaped or U-shaped opening direction of the third groove 53 and the U-shaped or U-shaped opening direction of the second groove 52 is greater than 0° and less than or equal to 90°. The metamaterial of one embodiment of the present invention, by staggering the openings of the three U-shaped or U-shaped grooves, can further broaden the bandwidth of spatial filtering.

[0075] In one embodiment, the U-shaped or U-shaped opening direction of the first groove 51 and the third groove 53 is perpendicular to the U-shaped or U-shaped opening direction of the second groove 52; further, the U-shaped opening direction of the first groove 51 is opposite to the U-shaped or U-shaped opening direction of the third groove 53, that is, the included angle between the two directions is 180°.

[0076] In one embodiment, the U-shaped first groove 51 includes a first groove 51a, a second groove 51b, and a third groove 51c connected in sequence. The first groove 51a and the third groove 51c are respectively connected to the two ends of the second groove 51b, and the included angles between the first groove 51a and the third groove 51c and the second groove 52 are both 80° to 100°. For example, the first groove 51a and the third groove 51c are both perpendicular to the second groove 51b.

[0077] In one embodiment, the length d of the first groove 51a is the same as the length of the second groove 51b and the third groove 51c, which is 0.9 to 1.4 mm.

[0078] In one embodiment, the first substrate 10 and / or the second substrate 20 are rectangular plates, or more specifically, square plates, with a side length of 5 to 8 mm, for example, 7 mm.

[0079] In one embodiment, the thickness of the first substrate 10 and the second substrate 20 can be 1.2 to 1.8 mm, for example 1.5 mm.

[0080] In one embodiment, the first substrate 10 and the second substrate 20 are identical, that is, they have the same shape, size, etc.

[0081] In one embodiment, the dielectric constant of the first substrate 10 and / or the second substrate 20 may be 3 to 50.

[0082] In one embodiment, the first substrate 10 and / or the second substrate 20 may be one or more of ceramic fiber cloth, glass fiber board, aluminum silicate fiber cotton, and alumina fiber cotton.

[0083] In one embodiment, the first substrate 10 and / or the second substrate 20 can withstand temperatures of 1000 to 1200°C.

[0084] One embodiment of the present invention provides a method for preparing the above-mentioned metamaterial, comprising:

[0085] A dihydrogen phosphate complex is provided, comprising a dihydrogen phosphate, a titanate or barium lanthanum titanium, and a solvent;

[0086] Using a dihydrogen phosphate complex as a raw material, multiple pre-formed microstructures are formed on at least one substrate to obtain a pre-formed metamaterial; and

[0087] The pre-formed metamaterial is sintered to obtain the metamaterial.

[0088] In one embodiment, the solvent is water.

[0089] In one embodiment, the mass ratio of dihydrogen phosphate, titanate (or barium lanthanum titanium) and solvent is dihydrogen phosphate: titanate (or barium lanthanum titanium): solvent = (1-3):1:1.

[0090] In one embodiment, multiple pre-formed microstructures can be formed on a substrate by screen printing, embossing, or inkjet printing.

[0091] In one embodiment, the preformed metamaterial can be dried at a stepped temperature, the drying process at the stepped temperature including:

[0092] Keep warm at 80-90℃ for 4-6 hours. The temperature can be, for example, 82℃, 85℃, or 88℃, and the time can be, for example, 4.5 hours, 5 hours, or 5.5 hours.

[0093] Afterwards, keep warm at 90-100℃ for 3-5 hours. The temperature can be, for example, 92℃, 95℃, or 98℃, and the time can be, for example, 3.5 hours, 4 hours, or 4.5 hours.

[0094] Finally, keep warm at 100-200℃ for 2-3 hours. The temperature can be, for example, 110℃, 120℃, 130℃, 140℃, 150℃, 160℃, 170℃, 180℃, or 190℃, and the time can be, for example, 2.5 hours.

[0095] In one embodiment, the pre-formed metamaterial can be aligned and pressed to obtain a pre-formed multilayer metamaterial structure layer, and then the pre-formed metamaterial structure layer can be sintered to produce a multilayer metamaterial structure layer.

[0096] In one embodiment, the preformed metamaterial is sintered using LTCC stepped high-temperature sintering, wherein LTCC stepped high-temperature sintering includes:

[0097] Raise the temperature from 20-30℃ to 300-500℃ (e.g., 3℃ / min, 4℃ / min) at a heating rate of 2-5℃ / min (e.g., 3℃ / min, 4℃ / min) and hold for 4-6 hours;

[0098] Raise the temperature from 300–500°C to 500–800°C (e.g., 520°C, 550°C, 580°C, 600°C, 620°C, 650°C, 700°C, 750°C) at a heating rate of 5–8°C / min (e.g., 6°C / min, 7°C / min) and hold for 3–5 hours; and

[0099] Raise the temperature from 500-800℃ to 800-1000℃ (e.g., 820℃, 850℃, 880℃, 900℃, 920℃, 950℃) at a heating rate of 10-15℃ / min (e.g., 12℃ / min, 13℃ / min) and hold for 2-3 hours.

[0100] One embodiment of the present invention provides a metamaterial that can be used in antennas and radomes.

[0101] The metamaterial of one embodiment of the present invention, compared with existing metal microstructure metamaterials, not only has superior electromagnetic and self-adhesive properties, but also good high-temperature stability and chemical stability. It can overcome the technical defects of existing metal microstructures such as complex processing, wrinkling, high-temperature oxidation, and introduction of other adhesives, so that it can be widely used in the fields of antennas, radomes and other technologies.

[0102] The metamaterial of one embodiment of the present invention employs an artificial microstructure of dihydrogen phosphate composite, which can achieve the functions of an equivalent metallic microstructure metamaterial and possesses excellent electromagnetic response. For example, it can broaden the spatial filtering bandwidth through a multi-layer groove-circular hole array, achieve large-angle wave transmission through a square array structure, achieve wave transmission and stealth integration through a double-layer Y-shaped structure, and achieve beam deflection through a multi-layer gradient ring structure. Furthermore, the fabrication process of the dihydrogen phosphate composite artificial microstructure is simple, significantly reducing the production cost of the product and improving its overall competitiveness.

[0103] One embodiment of the present invention can achieve different electromagnetic effects by adjusting the composition, shape, size, and different interlayer structure designs and proportions of the artificial microstructure of the dihydrogen phosphate composite metamaterial, thus enabling it to have a wide range of applications.

[0104] The metamaterial of one embodiment of the present invention exhibits significantly increased transmittance in the high-frequency band and a slight increase in transmittance in the low-frequency band compared to conventional metamaterials. For example, the electromagnetic transmittance bandwidth of conventional structures is less than 1 dB, ranging from 8.4 to 11.2 GHz, while the metamaterial of one embodiment of the present invention can reach 7.6 to 11.4 GHz.

[0105] The metamaterial and its preparation method according to an embodiment of the present invention will be further described below with reference to the accompanying drawings and specific embodiments.

[0106] Example 1

[0107] S1: Prepare a composite slurry of aluminum dihydrogen phosphate, deionized water, and strontium titanate in a mass ratio of 1:1:1, wherein the dielectric constant of strontium titanate is 200.

[0108] S2: The screen designed according to the predetermined function is placed on the screen printing machine, and then the dihydrogen phosphate composite paste is printed onto the first substrate 10 through the screen printing machine to form an array of square microstructures 31a (refer to...). Figure 5 The preformed metamaterial is obtained; wherein the first substrate 10 is a high-temperature resistant aluminum silicate cotton with a temperature resistance of over 1200℃.

[0109] S3: Place the first substrate 10 (pre-formed metamaterial) after screen printing in the oven and set the drying temperature curve, in which the substrate is kept at 80℃ for 4 hours, 100℃ for 3 hours, and 200℃ for 2 hours in sequence, and dried in step temperature order.

[0110] S4: Then, the baked substrate is placed in an LTCC sintering furnace, and a sintering temperature curve is set. The temperature is increased from room temperature to 300℃ at a heating rate of 3℃ / min and held for 4 hours. The temperature is increased from 300℃ to 500℃ at a heating rate of 6℃ / min and held for 3 hours. The temperature is increased from 500℃ to 800℃ at a heating rate of 10℃ / min and held for 2 hours. The first substrate 10 with microstructure is sintered through three temperature steps to obtain a metamaterial with square microstructure 31a.

[0111] Comparative Example 1

[0112] The designed and periodically arranged metallic metamaterial structure pattern (the same as the pattern in Example 1) is printed onto a film using a photoplotter. Photoresist is then applied to a copper-clad substrate (including epoxy resin board, polyimide film, etc.) obtained by thermal evaporation, sputtering, chemical deposition, or electron beam deposition. The printed film and the photoresist-coated substrate are then aligned and bonded together. The substrate is exposed to ultraviolet light using a photolithography machine, followed by development, chemical etching, and film removal to obtain the metallic metamaterial structure.

[0113] The metallic metamaterial prepared in Comparative Example 1 and the dihydrogen phosphate metamaterial prepared in Example 1 were respectively loaded onto a ceramic plate for electromagnetic wave transmittance testing. The results are as follows: Figures 10a to 10i As shown in the figure, the metamaterial of Example 1 can achieve anti-reflection effect on a flat plate under large incident angles within the range of 10-18 GHz. At the same time, the larger the incident angle, the more obvious the anti-reflection effect of the metamaterial structure on the flat plate, and even the minimum point improvement can reach more than 2 dB when the incident angle is 70-80°.

[0114] Example 2

[0115] S1: A sodium dihydrogen phosphate composite slurry is prepared by mixing sodium dihydrogen phosphate, deionized water, and barium strontium titanate in a mass ratio of 1:1:1, wherein the dielectric constant of barium strontium titanate is 350. Barium strontium titanate comprises strontium carbonate, barium carbonate, titanium dioxide, strontium titanate, and Ba-Al-Si glass powder in a mass ratio of 2:2:4:1:1.

[0116] S2: The screen designed according to the predetermined function is placed on the screen printing machine, and then the dihydrogen phosphate composite paste is printed onto the first substrate 10 through the screen printing machine to form an array of Y-shaped microstructures 31b (refer to...). Figure 6 , 7 The preformed metamaterial is obtained; wherein the first substrate 10 is a ceramic fiber cloth with a temperature resistance of over 1000℃.

[0117] S3: Place the screen-printed substrate (pre-formed metamaterial) in the oven and set the drying temperature curve, in which the substrate is kept at 80℃ for 3 hours, 100℃ for 3 hours, and 200℃ for 2 hours in sequence, and dried in step temperature order.

[0118] Repeat step S2 on the other side of the baked substrate to screen print the metamaterial structure pattern on the other side, and then dry the screen-printed metamaterial according to step S3.

[0119] S4: Then, the baked substrate is placed in an LTCC sintering furnace, and a sintering temperature profile is set. The temperature is increased from room temperature to 300℃ at a heating rate of 5℃ / min and held for 4 hours. The temperature is increased from 300℃ to 500℃ at a heating rate of 8℃ / min and held for 3 hours. The temperature is increased from 500℃ to 800℃ at a heating rate of 10℃ / min and held for 2 hours. The substrate with microstructure is sintered through three temperature steps to obtain a metamaterial with Y-shaped microstructure 31b.

[0120] The dihydrogen phosphate metamaterial prepared in Example 2 was loaded onto a ceramic plate, and its electrical properties were tested. The results are as follows: Figure 11 As shown. From Figure 11As can be seen, the metamaterial structure prepared in Example 2 can achieve good wave transmission in the X-band and Ku-band in the 8-18 GHz range, while having good wave absorption characteristics near 13.5 GHz and 15 GHz, and good reflection characteristics at 17 GHz.

[0121] Example 3

[0122] S1: Magnesium dihydrogen phosphate, barium lanthanum titanium, and deionized water are mixed in a mass ratio of 1:1.5:1 to prepare a dihydrogen phosphate composite slurry, wherein the dielectric constant of barium lanthanum titanium is 90.

[0123] S2: The screen designed according to the predetermined function is placed on the screen printing machine, and then the dihydrogen phosphate composite paste is printed onto the first substrate 10 through the screen printing machine to form a ring-shaped microstructure 31c with phase gradient arrangement (refer to...). Figure 8 , 9 The preformed metamaterial is obtained; wherein the first substrate 10 is an alumina fiber cloth with a temperature resistance of over 1000℃.

[0124] S3: Place the screen-printed substrate (pre-formed metamaterial) in the oven and set the drying temperature curve, in which the substrate is kept at 85℃ for 2 hours, 100℃ for 3 hours, and 150℃ for 2 hours in sequence, and dried in the order of the temperature steps.

[0125] Repeat steps S2 and S3 to screen print multilayer metamaterials and dry them. Then, align and bond the dried metamaterials to form a multilayer metamaterial structure.

[0126] S4: Then, the laminated multilayer substrate is placed in an LTCC sintering furnace, and a sintering temperature profile is set. The temperature is increased from room temperature to 400℃ at a heating rate of 3℃ / min and held for 2 hours. The temperature is increased from 400℃ to 600℃ at a heating rate of 8℃ / min and held for 2 hours. The temperature is increased from 600℃ to 900℃ at a heating rate of 12℃ / min and held for 2 hours. The substrate with the ring-shaped microstructure is sintered through three temperature steps to obtain a metamaterial with a gradient ring-shaped microstructure 31c.

[0127] The dihydrogen phosphate metamaterial prepared in Example 3 was loaded onto an antenna, and radiation pattern tests were performed. The results are as follows: Figure 12 As shown. In Figure 12 In the text, "antenna" indicates that the transmittance test only involved the antenna, while "antenna + dihydrogen phosphate metamaterial" indicates that the transmittance test included both the antenna and dihydrogen phosphate material. Figure 12 It can be seen that the metamaterial structure prepared in Example 3 can achieve a beam deflection of 9° when incident at 0°.

[0128] Example 4

[0129] The metamaterial of this embodiment includes a first substrate 10, a second substrate 20, a first microstructure layer, a second microstructure layer, and a third microstructure layer. The first substrate 10 includes a first surface 11 and a second surface disposed opposite to the first surface 11. The first surface 11 and the second surface are planes perpendicular to the thickness direction of the first substrate 10. The first microstructure layer is disposed on the first surface 11 and includes a plurality of first microstructures 31 (5×5) arranged in a square array. The second microstructure layer is disposed on the second surface and includes a plurality of second microstructures 32 arranged in a square array.

[0130] The second substrate 20 includes a third surface and a fourth surface 21 disposed opposite to the third surface. The third surface is disposed on the second surface of the first substrate 10, that is, the third surface is in contact with the second surface, so that the second microstructure layer is sandwiched between the second surface and the third surface. The first surface 11 and the fourth surface 21 are two surfaces of the metamaterial disposed opposite to each other, and the third microstructure layer is disposed on the fourth surface 21.

[0131] The third microstructure layer includes a plurality of third microstructures 33 arranged in a square array. The number of third microstructures 33 is the same as that of the first microstructures 31 and the second microstructures 32. The third microstructures 33 have the same shape and size as the first microstructures 31 and the second microstructures 32, and the material is the same as that of the microstructures in Embodiment 1. At the same time, each third microstructure 33 is arranged opposite to one first microstructure 31 and one second microstructure 32. That is, along the thickness direction of the first substrate 10, the projections of the first microstructure layer, the second microstructure layer and the third microstructure layer completely overlap.

[0132] The metamaterial has multiple circular first through-holes 41 and circular second through-holes 42. A coating formed of the dihydrogen phosphate material of Example 1 is deposited on the sidewalls of both the first through-holes 41 and 42. The first through-holes 41 and 42 have the same radius. Each first through-hole 41 and each second through-hole 42 are interconnected, and the interconnected first through-holes 41 and 42 have the same axis, which is perpendicular to the first substrate 10 and the second substrate 20. Each first through-hole 41 penetrates a first microstructure 31, the first substrate 10, and a second microstructure 32. Each second through-hole 42 penetrates the second substrate 20 and a third microstructure 33. That is, the number of first through-holes 41 and 42 is the same as the number of first microstructures 31, 32, and 33. The radius of each first through-hole 41 and 42 is 0.20 mm, and the side lengths of each first microstructure 31, 32, and 33 are 3.5 mm.

[0133] Each of the first microstructure 31, the second microstructure 32, and the third microstructure 33 has a U-shaped first groove 51, a second groove 52, and a third groove 53 (see reference). Figures 6 to 9 (As shown), and the first groove 51, the second groove 52, and the third groove 53 have the same structure and dimensions; refer to Figure 9 The first groove 51 is composed of a first groove 51a, a second groove 51b, and a third groove 51c. The first groove 51a and the third groove 51c are perpendicular to the second groove 51b. The length d of the first groove 51a is 1 mm, and the width w is 0.12 mm. The opening direction of the first groove 51 is perpendicular to the opening direction of the second groove 52 and opposite to the opening direction of the third groove 53.

[0134] Comparative Example 2

[0135] The difference between the metamaterial in this example and that in Example 4 is that the substrate used in this example is a single-layer substrate, the first microstructure is a regular rectangular metal patch without grooves, and the first microstructure is connected to the metal ground of the second microstructure through a metal via.

[0136] Comparative Example 3

[0137] The metamaterial in this example has the same structure as that in Example 4, except that the material of the microstructure and the coating material in the first through hole 41 and the second through hole 42 in this example are both metallic copper.

[0138] The metamaterials of Example 4, Comparative Example 2, and Comparative Example 3 were tested for wave transmittance under the same conditions. For specific results, please refer to [link to relevant documentation]. Figure 13a and 13b .from Figure 13a , 13b It can be seen that the metamaterial of Example 4 has a significantly increased transmittance in the high-frequency band compared to the metamaterial of Comparative Example 2, and the transmittance in the low-frequency band has also increased slightly. Moreover, the electromagnetic transmittance bandwidth of the metamaterial of Comparative Example 2 (less than 1 dB) is 8.4 to 11.2 GHz, the electromagnetic transmittance bandwidth of the metamaterial of Comparative Example 3 is 8.2 to 11.4 GHz, and the electromagnetic transmittance bandwidth of the metamaterial of Example 4 can reach 7.6 to 11.4 GHz. The metamaterial of Example 4 has the same effect of broadening the spatial filtering bandwidth as the metallic metamaterial.

[0139] The above description is only a preferred embodiment of the present invention, but the scope of protection of the present invention is not limited thereto. Any changes or substitutions that can be easily conceived by those skilled in the art within the scope of the technology disclosed in the present invention should be included within the scope of protection of the present invention.

Claims

1. A metamaterial, comprising: At least one substrate; as well as At least one microstructure layer is disposed on the at least one substrate; Wherein, the at least one microstructure layer includes multiple microstructures, and the material of the multiple microstructures includes a dihydrogen phosphate complex, wherein the dihydrogen phosphate complex includes dihydrogen phosphate and titanate or barium lanthanum titanium; The mass ratio of the dihydrogen phosphate to the titanate or the barium lanthanum titanium is 1:1 to 1:

3. And / or, the dielectric constant of the titanate or the barium lanthanum titanium is 30 to 500; The at least one substrate includes a first substrate, the first substrate including a first surface and a second surface disposed opposite to the first surface; the at least one microstructure layer includes a first microstructure layer and a second microstructure layer; the first microstructure layer is disposed on the first surface and includes one or more first microstructures; the second microstructure layer is disposed on the second surface and includes one or more second microstructures. One or more first through-holes are provided in the metamaterial, each first through-hole penetrating a first microstructure, a first substrate, and a second microstructure; and / or, The at least one substrate further includes a second substrate, and the at least one microstructure layer further includes a third microstructure layer; the third microstructure layer includes one or more third microstructures; the second substrate includes a third surface and a fourth surface disposed opposite to the third surface, the third surface is disposed on the second surface of the first substrate, and the second microstructure layer is sandwiched between the second surface and the third surface; the third microstructure layer is disposed on the fourth surface; One or more second through holes are formed on the second substrate and the third microstructure layer, each second through hole penetrating the second substrate and the third microstructure, and each second through hole communicating with a first through hole; A groove is formed on each of the first microstructure, each of the second microstructure, and each of the third microstructures; a third groove is formed on each third microstructure, and the third groove penetrates the third microstructure along its thickness direction; the first groove, the second groove, and the third groove are U-shaped or U-shaped; the angle between the U-shaped or U-shaped opening direction of the first groove and the U-shaped or U-shaped opening direction of the second groove is greater than 0° and less than or equal to 90°, and the angle between the U-shaped or U-shaped opening direction of the third groove and the U-shaped or U-shaped opening direction of the second groove is greater than 0° and less than or equal to 90°; The metamaterial has self-adhesive properties, and achieves wide spatial filtering bandwidth through a multi-layer groove-circular hole array, large-angle wave transmission through a square array structure, wave transmission and stealth integration, and beam deflection through a multi-layer gradient circular ring structure.

2. The metamaterial according to claim 1, wherein, The dihydrogen phosphate salt includes one or more of aluminum dihydrogen phosphate, magnesium dihydrogen phosphate, sodium dihydrogen phosphate, and disodium hydrogen phosphate; and / or, The titanate includes one or more of strontium titanate, barium titanate, calcium titanate, and magnesium titanate.

3. The metamaterial according to claim 1, wherein, A first groove is formed on each of the first microstructures, a second groove is formed on each of the second microstructures, and a third groove is formed on each of the third microstructures; and / or, The angle between the axis of the first through hole, the axis of the second through hole and the first surface and / or the second surface is 85° to 95°.

4. A method for preparing a metamaterial according to any one of claims 1 to 3, comprising: A dihydrogen phosphate complex is provided, the dihydrogen phosphate complex comprising a dihydrogen phosphate, a titanate or barium lanthanum titanium, and a solvent; Using the aforementioned dihydrogen phosphate complex as raw material, a plurality of pre-formed microstructures are formed on at least one substrate to obtain a pre-formed metamaterial. as well as The preformed metamaterial is sintered to obtain the metamaterial.

5. The preparation method according to claim 4, comprising drying the preformed metamaterial at a stepped temperature, wherein the drying at the stepped temperature includes: Keep warm at 80-90℃ for 4-6 hours, at 90-100℃ for 3-5 hours, and at 100-200℃ for 2-3 hours.

6. The preparation method according to claim 5, comprising subjecting the pre-formed metamaterial after drying to a stepped high-temperature sintering treatment, wherein the stepped high-temperature treatment includes: The temperature is increased from 20-30℃ to 300-500℃ at a heating rate of 2-5℃ / min and held for 4-6 hours. Then the temperature is increased from 300-500℃ to 500-800℃ at a heating rate of 5-8℃ / min and held for 3-5 hours. Finally, the temperature is increased from 500-800℃ to 800-1000℃ at a heating rate of 10-15℃ / min and held for 2-3 hours.

Citation Information

Patent Citations

  • Metamaterial and method for producing metamaterial function board

    CN102476957A

  • High-temperature-resistant printing material and application thereof

    CN107311465A

  • Artificial magnetic conductor reflection plate for five-band multiplexing

    CN107394412A