Method for producing curved laminated glazing

By depositing an enamel layer containing zinc oxide particles on the glass sheet and dissolving the thin layer stack during the firing process, the problem of reduced adhesion and changes in optical appearance caused by the interaction of the enamel layer and the thin layer stack is solved, Improved optical properties and mechanical strength of curved laminated glazing units.

CN116348428BActive Publication Date: 2024-10-22SAINT-GOBAIN SAFETY GLASS CO FRANCE
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202280006902.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2021-10-12
Filing Date
2022-10-10
Publication Date
2024-10-22
Estimated Expiration
2042-10-10

AI Technical Summary

Technical Problem

In curved laminated glazing units, when enamel layers and thin-layer stacks are arranged on the same side, undesirable interactions tend to occur, leading to a reduction in the adhesion of the enamel and a change in the optical appearance, especially in the case of bismuth-containing enamels and Bubbles appear at the interface formed between the nitride layers, affecting their chemical resistance and aesthetic appearance.

Method used

An enamel composition containing 1-15% by weight of zinc oxide particles is deposited on the glass sheet by screen printing, ensuring that the enamel layer faces the lamination intermediate layer, taking advantage of the particle size distribution of the zinc oxide particles (d90 up to 5 μm) to reduce mechanical brittleness oxidizes and improves optical properties while dissolving thin layer stacks during firing to avoid bonding issues.

Benefits of technology

It effectively reduces the risk of glass sheets bonding during the bending process, improves the optical properties and mechanical strength of the enamel paint, and maintains the aesthetic appearance and chemical resistance of the enamel paint layer.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116348428B_ABST
    Figure CN116348428B_ABST
Patent Text Reader

Abstract

The invention relates to a method for obtaining a laminated curved glazing unit, wherein (a) a first glass sheet (10) is provided, coated on at least a portion of one of its faces with a stack of thin layers (12), then (b) an enamel layer (14) is deposited on a portion of the surface of the stack of thin layers (12) by screen printing an enamel composition containing 1 to 15% by weight of zinc oxide particles, the zinc oxide particles having a volume particle size distribution such that the d90 is at most 5 μm. After lamination (d) with an additional glass sheet (20), the enamel layer (14) is turned towards a laminating interlayer (30).
Need to check novelty before this filing date? Find Prior Art

Description

[0001] The invention relates to the field of curved laminated glazing units for motor vehicles, for example for roofs or windscreens, comprising a glass sheet coated with a stack of thin layers and enamel layers.

[0002] Laminated glazing units are glazing units in which two glass sheets are adhesively bonded using a laminating interlayer. The laminating interlayer can in particular retain glass fragments in the event of breakage, but it also provides other functions, in particular with regard to breakage resistance or improved acoustic properties.

[0003] These glazing units often include various types of coatings intended to impart different properties.

[0004] The enamel layer, which is usually black and opaque, is usually deposited in the form of a peripheral band on a portion of the glazing unit that is intended to conceal and protect from UV radiation, and a polymer seal is used to secure and position the glazing unit to the window of the vehicle body. The enamel area also hides the area for securing the interior rearview mirror and various connectors and sensors.

[0005] In laminated glazing units, these enamel layers are usually arranged on face 2, which is conventionally numbered starting from the face intended to be positioned on the outside of the vehicle. Face 2 is therefore the face in contact with the laminating interlayer. The aesthetic appearance of the enamel layer, as viewed from the outside of the vehicle, has always been of particular importance to automobile manufacturers. The enamel is usually obtained by firing a composition comprising glass frit and pigment at a temperature above 500° C. The glass frit comprises fine particles of glass with a low melting point, which soften and adhere to the glass sheet under the effect of the firing heat treatment. A generally opaque mineral layer is thereby formed, which has a high chemical and mechanical strength and adheres well to the glass while retaining the pigment particles. The firing step is usually carried out simultaneously with the bending of the glass sheet.

[0006] In the case of laminated glazing unit production, the two glass sheets of the glazing unit are usually bent together, wherein the glass sheet intended to be positioned on the inside of the vehicle is usually arranged above the other glass sheet carrying the enamel. In other processes, each glass sheet is bent separately. In all cases, the enamel must have non-stick properties in order to prevent any adhesion between the two glass sheets or between a glass sheet and a bending tool during the bending process. For this purpose, bismuth-containing enamels are usually used, which are obtained from glass frits containing bismuth oxides.

[0007] The coating, usually in the form of a stack of thin layers, may also be present on one of the glass sheets of the laminated glazing. These may in particular be conductive layers, which can provide two types of functions. On the one hand, the conductive layer can dissipate heat by the Joule effect when it is planned to provide an electric current. This is a layer used for heating, which can be used for example for defrosting or defogging. On the other hand, due to the reflection of infrared radiation by these layers, they have the properties of solar control or low emissivity. The value of the layers is that they provide an improvement in thermal comfort or energy saving, while reducing the consumption intended for heating or air conditioning. These stacks of layers are usually arranged on face 3 of the laminated glazing unit and are therefore also in contact with the laminating interlayer.

[0008] However, in some cases described below, it is interesting to arrange the stack of enamel layer and thin layer on the same glass sheet and therefore on the same face of the glass sheet in question so that these coatings are protected on the inside of the laminated glazing.

[0009] However, it has been observed that when a glass sheet coated with a thin layer of a multilayer has to be provided with an enamel layer, undesirable interactions can occur between the multilayer and the enamel in the event of bending, leading in particular to a deterioration of the aesthetic appearance of the enamel. In particular, it has been observed that, in particular when the multilayer contains at least one layer of nitride and the enamel contains bismuth, bubbles formed in the enamel close to the interface between it and the multilayer lead to a significant reduction in the adhesion of the enamel, changes in its optical appearance (in particular the color on the glass side, i.e. on the side opposite to the enamel) and a reduction in its chemical resistance, in particular its acid resistance.

[0010] Several solutions to this problem have been proposed.

[0011] The stack of thin layers can be removed beforehand at the location where the enamel layer is deposited, for example by an abrasive tool, so that the enamel is deposited in direct contact with the glass sheet and any adhesion problems between the enamel layer and the stack of thin layers are avoided. However, mechanical abrasion produces visible scratches, including on the enamel layer.

[0012] Application WO2014 / 133929 and the earlier application WO0029346 proposed the concept of using special glass frits for enamels that are able to dissolve the stack of thin layers during firing or pre-firing, thereby becoming directly attached to the glass. However, these enamels do not have good anti-adhesive properties and cause the two glass sheets to stick together during bending.

[0013] Application WO 2019 / 106264 proposes to modify the stack of thin layers by adding an oxide layer between the stack and the enamel containing bismuth. However, such a modification is not always possible.

[0014] The object of the present invention is to overcome these disadvantages.

[0015] To this end, the subject of the invention is a method for obtaining a curved laminated glazing unit, in particular for a windshield or a roof of a motor vehicle, comprising the following successive steps:

[0016] a. providing a first glass sheet, having a stack of thin layers covering at least a portion of one of its surfaces,

[0017] b. a step of depositing an enamel layer on a portion of the surface of the stack of thin layers, the deposition being carried out by screen printing an enamel composition comprising 1 to 15% by weight of zinc oxide particles having a volume particle size distribution such that d90 is at most 5 μm,

[0018] c. a step of bending the first glass sheet, at least at the end of which the stack of thin layers below the enamel layer is completely dissolved by the enamel layer, and then

[0019] d. The step of laminating the first glass sheet with an additional glass sheet by laminating an interlayer so that the enamel layer faces the interlayer.

[0020] Another subject of the invention is a curved laminated glazing unit obtained or obtainable by the process, in particular for a windscreen or roof of a motor vehicle, comprising a first glass sheet covered on at least a portion of one of its faces with a stack of thin layers, coated on a portion of its surface with an enamel layer comprising zinc oxide particles having a volume particle size distribution such that the d90 is at most 5 μm, the first glass sheet being laminated with an additional glass sheet via a laminating interlayer, the enamel layer facing the laminating interlayer.

[0021] The use of zinc oxide particles can reduce the mechanical embrittlement of the glass by the enamel and can improve the optical properties of the enamel while reducing the risk of sticking during bending between the two glass sheets or between the glass sheet and the bending tool (depending on the bending method used).

[0022] In this document, the stack of thin layers and the enamel layer are collectively referred to as a "coating".

[0023] Step a

[0024] The first glass sheet can be flat or curved. During the deposition of the stack of thin layers and then the deposition of the enamel layer, the first glass sheet is usually flat and then it is bent during step c. The first glass sheet is thus bent into a curved laminated glazing unit according to the invention.

[0025] The glass of the first glass sheet is typically soda-lime-silica glass, but other glasses such as borosilicates or aluminosilicates may also be used.The first glass sheet is preferably obtained by the float process, ie by a process comprising pouring molten glass onto a bath of molten tin.

[0026] The first glass sheet can be made of transparent glass or colored glass, preferably of colored glass, for example green, gray or blue. For this purpose, the chemical composition of the first glass sheet advantageously contains iron oxide in an amount of 0.5-2% by weight. It may also contain other colorants, such as, for example, cobalt oxide, chromium oxide, nickel oxide, erbium oxide or selenium.

[0027] The thickness of the first glass sheet preferably lies in the range of 0.7 to 19 mm, in particular 1 to 10 mm, in particular 2 to 6 mm, or even 2 to 4 mm.

[0028] The lateral dimensions of the first glass sheet (and the additional glass sheet) will be adapted to the lateral dimensions of the laminated glazing unit into which they are intended to be integrated. The surface area of ​​the first glass sheet (and / or the additional glass sheet) is preferably at least 1 m 2 .

[0029] The first glass sheet is preferably coated with the multilayer of thin layers over at least 70% of the surface of the face of the glass sheet, in particular at least 90% of the surface, or even over the entire surface. Some areas may be uncovered in order to arrange communication windows allowing waves to pass.

[0030] Preferably, the stack is coated with an enamel layer over 2 to 25%, in particular 3 to 20%, or even 5 to 15% of its surface. The enamel layer preferably comprises a peripheral band, i.e. a separate band, which, at any point on the periphery of the first glass sheet, extends inwards towards the first glass sheet over a width which is generally variable and which is typically 1 to 20 cm, depending on the area of ​​the final glazing.

[0031] The stack of thin layers is preferably in contact with the inner glass sheet.When deposited, the enamel layer is preferably in contact with the stack of thin layers.

[0032] In this context, "contact" is intended to mean physical contact. The expression "based on" is preferably intended to mean the fact that the layer in question comprises at least 50% by weight of the material in question, in particular 60% by weight, or even 70% by weight and even 80% by weight or 90% by weight. The layer may even consist essentially of this material or may consist of this material. "Essentially consisting of" is understood to mean that the layer may contain impurities that have no effect on its properties. The term "oxide" or "nitride" does not necessarily mean that the oxide or nitride is stoichiometric. In fact, they may be substoichiometric, superstoichiometric or stoichiometric.

[0033] The stack preferably comprises at least one nitride-based layer. The nitride is in particular a nitride of at least one element selected from aluminum, silicon, zirconium, titanium. It may contain nitrides of at least two or three of these elements, for example silicon zirconium nitride or silicon aluminum nitride. The nitride-based layer is preferably a silicon nitride-based layer, more particularly a layer consisting essentially of silicon nitride. When the silicon nitride layer is deposited by cathode sputtering, it usually contains aluminum, since it is common practice to dope the silicon target with aluminum to accelerate the deposition rate.

[0034] The nitride-based layer preferably has a physical thickness of 2 to 100 nm, in particular 5 to 80 nm.

[0035] Nitride-based layers are often used for stacks of a large number of thin layers, since they have advantageous barrier properties, since they prevent oxidation of other layers present in the stack, in particular of the functional layers to be described below.

[0036] Preferably, the stack comprises at least one functional layer, in particular an electrically conductive functional layer. The functional layer is preferably comprised between two thin dielectric layers, at least one of which is a nitride-based layer. Other possible dielectric layers are layers of, for example, oxides or oxynitrides.

[0037] The at least one electrically conductive functional layer is advantageously selected from:

[0038] - a metal layer, in particular a layer of silver, niobium or even gold, and

[0039] - a layer of a transparent conductive oxide, in particular selected from the group consisting of indium tin oxide, doped tin oxide (for example doped with fluorine or antimony) and doped zinc oxide (for example doped with aluminum or gallium).

[0040] These layers are particularly valuable due to their low emissivity, which gives the glazing unit excellent insulating properties. In glazing units for equipping land vehicles, especially motor vehicles, trains and also aircraft or sea vessels, low-emissivity glazing units can reflect part of the solar radiation outwards in hot weather and thus limit the heating of the passenger compartment of the vehicle and, where appropriate, reduce air conditioning costs. Conversely, in cold weather, these glazing units can keep the heat in the passenger compartment and thus reduce the required thermal energy. The same applies to the case of glazing units for equipping buildings.

[0041] According to a preferred embodiment, the stack of thin layers comprises at least one silver layer, in particular one, two, three or even four silver layers. The physical thickness of the silver layers, or where appropriate the sum of the thicknesses of the silver layers, is preferably 2-50 nm, in particular 3-40 nm.

[0042] According to another preferred embodiment, the stack of thin layers comprises at least one layer of oxides of indium and tin. Its physical thickness is preferably from 30 to 200 nm, in particular from 40 to 150 nm.

[0043] In order to protect the or each conductive thin layer (whether metallic or based on a transparent conductive oxide) during the bending step, each of these layers is preferably surrounded by at least two dielectric layers. The dielectric layers are preferably based on oxides, nitrides and / or oxynitrides of at least one element chosen from silicon, aluminum, titanium, zinc, zirconium and tin.

[0044] At least part of the stack of thin layers can be deposited by various known techniques, such as chemical vapor deposition (CVD), or by cathode sputtering, in particular assisted by a magnetic field (magnetron method).

[0045] The stack of thin layers is preferably deposited by cathode sputtering, in particular magnetron sputtering. In this method, a plasma is generated in a high vacuum close to a target containing the chemical element to be deposited. By bombarding the target, the active species of the plasma cause the element to flake off, which is deposited on the glass sheet to form the desired thin layer. When the layer is made of a material resulting from a chemical reaction between the element flake off from the target and the gas contained in the plasma, the method is called a "reactive" method. The main advantage of this method is that, by running the glass sheet continuously under various targets, usually in the same equipment, stacks of very complex layers can be deposited on the same production line.

[0046] The above examples have conductive and infrared reflective properties, which have uses for providing heating functions (defrosting, defogging) and / or thermal insulation functions.

[0047] When the stack of thin layers is intended to provide a heating function, an electric current supply must be provided. This can in particular be a strip of silver paste deposited by screen printing on the stack of thin layers at two opposite edges of the glass sheet.

[0048] Step b

[0049] In this document, "enamel composition" is used to describe the liquid composition used to deposit a wet enamel layer on the glass sheet during step b. The term "enamel layer" is used to describe the layer at each stage of the process, both the wet layer (before possible pre-firing, if required, and before drying) and the final layer (after firing).

[0050] In step b, the enamel layer is preferably deposited from an enamel composition comprising at least one pigment, at least one glass frit and zinc oxide particles. Like the enamel layer, the enamel composition preferably does not contain lead oxide.

[0051] The enamel composition also typically includes an organic medium, which is intended to facilitate application of the composition to a substrate and its temporary bonding to the substrate and, if necessary, to be removed during pre-firing or firing of the enamel. The medium typically includes solvents, diluents, oils and / or resins.

[0052] The glass frit is capable of dissolving the stack of underlying layers. Preferably, the glass frit is based on bismuth zinc borosilicate (or bismuth zinc borate). When it is desired that the enamel be capable of dissolving the stack of thin layers during pre-firing or firing, as described in more detail in the remainder of this document, the proportions of bismuth and / or boron are preferably higher than those in the glass frits commonly used, in order to make it more "aggressive" to the stack of layers.

[0053] The pigment preferably comprises one or more oxides selected from the group consisting of chromium oxides, copper oxides, iron oxides, manganese oxides, cobalt oxides and nickel oxides. These may be, for example, copper and / or iron chromates.

[0054] "Zinc oxide particles" refers to particles consisting of or consisting essentially of zinc oxide (possibly with impurities). Thus, the term does not include particles of glass frit, which may contain zinc oxide in its composition.

[0055] "d90" is generally understood to mean the value such that 90% (by volume) of the particles have a size smaller than this value. The volume size distribution of the particles is preferably determined by laser particle size analysis.

[0056] Preferably, the zinc oxide particles have a volume particle size distribution such that the d90 is at most 3 μm, in particular at most 1 μm.

[0057] Preferably, the zinc oxide particles have a volume particle size distribution such that d50 is from 200 to 900 nm, in particular from 300 to 800 nm.

[0058] The proportion of zinc oxide particles in the enamel composition is preferably from 2 to 10% by weight, in particular from 3 to 8% by weight.

[0059] Advantageously, the enamel composition also comprises a proportion by volume of at least 0.5% refractory particles having a diameter of at least 20 μm, but no particles having a diameter greater than 80 μm.

[0060] "Refractory particles" are particles whose morphology is not significantly affected during the bending process. These particles must have a melting or softening temperature that is much higher than the temperature experienced during the bending process and must not be dissolved by the glass frit. Refractory particles are especially based on metal oxides or metals. Metal oxides are especially simple oxides, such as aluminum oxide, titanium oxide or zirconium oxide, or composite oxides, such as high melting point glass frits or inorganic pigments (the latter are especially called "composite inorganic color pigments" or CICPs).

[0061] The presence of a sufficient proportion of "large" refractory particles (thus a size, also called diameter, of at least 20 μm) can also prevent the glass sheets from sticking together during the bending process, or from sticking to the bending tool. Due to their size, the large refractory particles produce a morphology during the bending process in which the particles form peaks with the molten or softened glass frit gathering in the valleys. This size of 20 μm and more is much larger than the sizes of conventionally used glass frits and pigments.

[0062] The volume fraction of refractory particles having a size (or diameter) of 20 μm and above is preferably determined by laser diffraction granulometry. This fraction is at least 0.5%, and preferably at least 1%, in particular at least 2% and even at least 3%.

[0063] Preferably, the enamel composition contains the abovementioned volume proportions of refractory particles having a diameter of at least 30 μm, in particular at least 40 μm, and even at least 50 μm.

[0064] Another method for easily detecting the presence of large particles is to measure the fineness of the particles using a Heckman gauge (or fineness meter). According to this method, the fineness of the enamel composition measured with a Heckman gauge is 20-80 μm, especially 40-60 μm.

[0065] Preferably, the enamel composition does not contain particles (refractory or non-refractory) having a diameter greater than 80 microns to allow for proper deposition by screen printing. The presence of such particles can be determined by laser diffraction particle size measurement or using a Heckman gauge.

[0066] The enamel layer is deposited by screen printing. To this end, a screen printing screen is placed on the glass sheet, the screen comprising meshes, some of which are closed, and then the enamel composition is deposited on the screen, followed by applying a scraper to force the enamel composition through the screen in areas where the meshes of the screen are not closed, thereby forming a wet enamel layer. In order to ensure uniform deposition of large refractory particles, when the enamel composition contains them, the mesh opening of the screen is preferably at least 40 μm, especially at least 60 μm, or even at least 70 μm. Large mesh openings will catch the particles and prevent them from being deposited uniformly, while too large mesh openings will lead to too high a enamel thickness, which can weaken the mechanical strength of the glass. The mesh openings are preferably at most 100 μm, especially at most 80 μm.

[0067] The thickness of the wet enamel layer is preferably from 15 to 40 μm, in particular from 20 to 30 μm.

[0068] Step b is preferably followed by a drying step, the purpose of which is to remove at least part of the solvent contained in the enamel composition. This drying is generally carried out at a temperature of 120-180°C.

[0069] Step c

[0070] Bending can be carried out in particular using gravity (the glass deforms under its own weight) or by pressing at temperatures typically between 550 and 650° C.

[0071] According to a first embodiment, the two glass sheets (the first glass sheet and the additional glass sheet) are bent separately. In this case, it is important to avoid any bonding between the first glass sheet and the bending tool.

[0072] According to a second embodiment, the first glass sheet and the additional glass sheet are bent together, with the enamel layer facing the additional glass sheet. In this case, it is important to avoid any bonding between the two glass sheets. The glass sheets are preferably kept apart by placing an interlayer powder between the glass sheets to ensure a gap of several tens of microns, typically 20 to 50 microns. The interlayer powder is based, for example, on calcium carbonate and / or magnesium carbonate. During the bending process, the inner glass sheet (intended to be positioned in the passenger compartment) is usually placed above the outer glass sheet. Therefore, during the bending step, the additional glass sheet is placed above the first glass sheet.

[0073] Preferably, after step c, the enamel layer is opaque and has a black hue. Its lightness L*, measured in reflection from the glass side, is preferably less than 5. It has been observed that the addition of zinc oxide particles can reduce the value of the lightness L* and thus obtain a darker black enamel.

[0074] As mentioned above, the enamel layer advantageously forms a band around the periphery of the first glass sheet. Thus, the enamel layer can conceal and protect the seal, the connecting element or the sensor from UV radiation.

[0075] Optional pre-firing step (b1)

[0076] The method preferably comprises, between step b) and step c), a step b1) of prefiring the enamel layer, during which the stack of thin layers underlying the enamel layer is at least partially dissolved by said enamel layer.

[0077] This step is particularly useful in the second embodiment described above, wherein the first glass sheet and the additional glass sheet are bent together, with the enamel layer facing the additional glass sheet.

[0078] Dissolving the stack of thin layers with the enamel prevents the above mentioned interactions. At least after the bending step (step c), the components of the stack are dissolved in the enamel layer which is in direct contact with the glass sheet.

[0079] If the enamel layer has not completely dissolved the stack of thin layers after the pre-firing, this complete dissolution is achieved during the bending process which completes the enamel firing.

[0080] The complete dissolution of the stack of thin layers can be observed in particular by electron microscopy. Electrical measurements, in particular the sheet resistance, also allow the dissolution of the stack to be determined.

[0081] The pre-firing step is preferably carried out at a temperature of 150-800°C, especially 500-700°C.

[0082] This pre-firing allows the removal of the organic medium, or generally of any organic components that may be present in the enamel layer.

[0083] During the pre-firing, the stack of thin layers is preferably at least partially dissolved by the enamel layer. Depending on the temperature used and the type of enamel or stack, the stack may even be completely dissolved by the enamel layer during the pre-firing process. Alternatively, it may only partially dissolve during the pre-firing process and then completely dissolve during the bending process (step c).

[0084] Step d

[0085] The lamination step can be carried out by treatment in an autoclave, for example at a temperature of 110 to 160° C. and at a pressure of 10 to 15 bar. Prior to the autoclave treatment, air trapped between the glass sheet and the laminating interlayer can be eliminated by calendering or by applying negative pressure.

[0086] As mentioned above, the additional sheet is preferably the inner sheet of the laminated glazing unit, ie the sheet located on the concave side of the glazing unit, intended to be located in the passenger compartment.The coating is therefore arranged on face 2 of the laminated glazing.

[0087] The additional glass sheet can be made of soda-lime-silica glass or borosilicate or aluminosilicate glass. It can be made of transparent or colored glass. Its thickness is preferably 0.5 to 4 mm, especially 1 to 3 mm.

[0088] According to a preferred embodiment, the additional glass sheet has a thickness comprised between 0.5 mm and 1.2 mm. The additional glass sheet is in particular made of sodium aluminosilicate glass, preferably chemically strengthened. The additional glass sheet is preferably the inner sheet of a laminated glazing. The invention is particularly useful for this type of construction, for which it is difficult to arrange a stack of thin layers on face 3. Chemical strengthening (also known as "ion exchange") consists in bringing the glass surface into contact with a molten potassium salt (e.g. potassium nitrate) in order to strengthen the surface of the glass by exchanging the ions of the glass (here sodium ions) with ions having a larger ionic radius (here potassium ions). This ion exchange allows compressive stresses to be formed on the glass surface and over a certain thickness. Preferably, the surface stress is at least 300 MPa, in particular 400 MPa, and even 500 MPa, and at most 700 MPa, and the thickness of the compression zone is at least 20 μm, typically 20 μm to 50 μm. The stress distribution can be determined in a known manner using a polarizing microscope equipped with a Babinet compensator. The chemical tempering step is preferably carried out at a temperature of 380-550° C. and for a duration of 30 minutes to 3 hours. Chemical strengthening is preferably carried out after the bending step but before the lamination step. The glazing unit obtained is preferably a motor vehicle windscreen, in particular a heated windscreen.

[0089] According to another preferred embodiment, the additional glass sheet carries, on the face opposite to the face facing the laminating interlayer (preferably face 4, the additional sheet being the inner sheet), a stack of additional thin layers, in particular a stack with low emissivity, comprising transparent conductive oxides, in particular oxides of indium and tin (ITO). The invention is also particularly useful for this type of construction for which it is difficult to arrange stacks of thin layers on both faces of the same glass sheet (faces 3 and 4). In this embodiment, the laminating interlayer and / or the additional glass sheet are preferably colored, the glass sheet with the coating can be made of transparent glass. The glazing unit obtained is preferably a motor vehicle roof.

[0090] As an example of the latter preferred embodiment, mention may be made of a laminated curved roof which, starting from the outside of the vehicle, comprises a transparent glass sheet coated on face 2 with a stack of thin layers comprising at least one silver layer followed by an enamel layer, a laminating interlayer made of PVB, preferably colored, and an additional glass sheet made of colored glass, which carries on face 4 a low-emissivity stack of thin layers, in particular based on ITO.

[0091] The laminating interlayer preferably comprises at least one polyvinyl acetal sheet, in particular polyvinyl butyral (PVB) sheet.

[0092] If desired, the laminating interlayer may be tinted or untinted to adjust the optical or thermal properties of the glazing unit.

[0093] The laminating interlayer may advantageously have sound-damping properties in order to absorb airborne or structure-borne sound. To this end, it may in particular consist of three polymer sheets, including two "outer" PVB sheets surrounding an inner polymer sheet, the inner polymer sheet optionally being made of PVB, having a lower hardness than the outer sheets.

[0094] The laminating interlayer may also have thermal insulation properties, in particular infrared radiation reflecting properties. To this end, it may comprise a coating of a thin layer with low emissivity, for example a coating comprising a thin layer of silver or a coating of alternating dielectric layers with different refractive indices, deposited on an inner PET sheet surrounded by two outer PVB sheets.

[0095] The thickness of the laminating interlayer is typically 0.3 to 1.5 mm, in particular 0.5 to 1 mm. The laminating interlayer may have a smaller thickness at the edge of the glazing unit than in the center of the glazing unit in order to prevent double images when using a head-up display (HUD). Example

[0096] The following exemplary embodiments combine Figure 1 The invention is illustrated in a non-limiting manner.

[0097] Figure 1 An embodiment of the method according to the invention is schematically illustrated. It shows a schematic cross section of a portion of a glass sheet and elements deposited on the glass sheet close to its periphery. The various elements are obviously not represented to scale in order to be able to visualize them.

[0098] In step a, a first glass sheet 10 coated with a thin-film stack 12 is provided, and then a portion of the stack 12 is coated with an enamel layer 14 (step b), in particular by screen printing.

[0099] The assembly is then subjected to a pre-firing (step b1 ) which, in the case shown, results in partial dissolution of the stack 12 by the enamel 14 .

[0100] Then, an additional glass sheet 20, here provided with a stack 22 of another thin layer, is placed on the first glass sheet 10 and the assembly is then bent (step c). The view shown is only a view of the end of the glass sheet, the bending is not shown here. The figure shows that after bending, the enamel 14 has completely dissolved the stack 12 of thin layers below.

[0101] In step d, the first glass sheet 10 coated with the thin-film stack 12 and the enamel layer 14 is joined to the additional glass sheet 20 coated with the additional stack 22 by means of a laminating interlayer 30. The figures here show each individual element in an exploded view.

[0102] First series of embodiments

[0103] The method used in the first series of embodiments corresponds to [ Figure 1 ] is the implementation scheme shown in ].

[0104] A 2.1 mm thick transparent glass sheet, previously coated by cathode sputtering with a stack of thin layers comprising three silver layers protected by layers of zinc oxide, silicon nitride and a NiCr barrier, was partially coated by screen printing with a layer of enamel having a wet thickness of 25 μm.

[0105] In addition to glass frit, black pigment and medium, the enamel composition contains 5 wt% of large refractory oxide particles with a size greater than 20 μm. In a first embodiment according to the invention, 5 wt% of ZnO particles (D90 < 1 μm) are also added to the enamel composition.

[0106] The enamel layer was deposited by screen printing and the enamel was then dried (150°C, 1 to 2 minutes) before pre-firing at about 650-680°C.

[0107] After pairing with an additional glass sheet of tinted soda-lime glass having a stack comprising an ITO layer on face 4 , the assembly was bent at over 600° C. for 350 to 500 seconds.

[0108] After firing, the appearance viewed from face 1 , more specifically the black color (illuminant D65, reference observer 10°), is evaluated by measuring the lightness L* in reflection.

[0109] In the case of the examples according to the invention, a value L* of 4.5 on average was obtained, in contrast to 5.1 for the comparative example (without ZnO particles). In contrast to the examples according to the invention, the comparative example also had a slight haze in reflection.

[0110] For the comparative example, approximately 25% of the glass was broken at the corners at the moment of bending, with adhesion being observed, as well as transfer of the enamel on the opposite glass. On the other hand, for the examples according to the invention, no breakage was observed.

[0111] The laminated glazing units were also subjected to a 3-point bending test. For the comparative example, the breaking force was 128 N, whereas for the example according to the invention it was 172 N. The values ​​given are average values ​​from samples of 20 glazing units.

[0112] Second series of embodiments

[0113] The embodiments of this second series of embodiments differ from those of the first series in that the bending of the two glass sheets is respectively carried out by pressing at a temperature of 610-630°C.

[0114] For the first series, in addition to glass frit, black pigment and medium, the enamel composition also contains 5% by weight of large refractory oxide particles with a size greater than 20 μm. In a second embodiment according to the invention, 5% by weight of ZnO particles (D90 < 1 μm) are also added to the enamel composition. The third embodiment according to the invention contains 10% by weight of such particles.

[0115] In the case of the comparative example (without ZnO particles), it was observed that the glass adhered to the bending tool. This was not the case for the examples according to the invention.

Claims

1. A method for obtaining a curved laminated glazing unit, said method comprising the following consecutive steps: a. providing a first glass sheet (10) having a thin layer of a stack (12) covered on at least a portion of one of its surfaces, b. a step of depositing an enamel layer (14) on a portion of the surface of the stack (12) of thin layers by screen printing an enamel composition comprising 1 to 15% by weight of zinc oxide particles having a volume particle size distribution such that d90 is at most 5 μm, c. a step of bending the first glass sheet (10), at least at the end of which the stack (12) of thin layers located below the enamel layer (14) is completely dissolved by the enamel layer (14), and then d. The step of laminating the first glass sheet (10) with an additional glass sheet (20) by laminating an intermediate layer (30) so that the enamel layer (14) faces the intermediate layer (30).

2. The method of claim 1, wherein the curved laminated glazing unit is for a windshield or a roof of a motor vehicle.

3. The method according to claim 1, wherein the stack (12) of thin layers comprises at least one functional layer. The method according to claim 3 , wherein the at least one functional layer is a conductive functional layer. 5 . The method according to claim 4 , wherein the electrically conductive functional layer is selected from a metal layer, and a layer of a transparent conductive oxide. The method according to claim 4 , wherein the conductive functional layer is selected from a silver layer or a niobium layer.

7. The method of claim 4, wherein the conductive functional layer is selected from the group consisting of indium tin oxide, doped tin oxide, and doped zinc oxide.

8. The method according to claim 1, such that after step d, the enamel layer (14) is opaque, has a black hue, and forms a band around the periphery of the first glass sheet (10).

9. The method of claim 1, wherein the zinc oxide particles have a volume particle size distribution such that d90 is at most 1 μm.

10. The method of claim 1, wherein the zinc oxide particles have a volume particle size distribution such that d50 is from 200 nm to 900 nm.

11. The method of claim 1, wherein the zinc oxide particles have a volume particle size distribution such that d50 is from 300 nm to 800 nm.

12. The method according to claim 1, wherein the proportion of zinc oxide particles in the enamel composition is 2-10 wt%.

13. The method according to claim 1, wherein the proportion of zinc oxide particles in the enamel composition is 3-8% by weight.

14. The method of claim 1, wherein the enamel composition further comprises at least 0.5% by volume of refractory particles having a diameter of at least 20 μm, but no particles having a diameter greater than 80 μm.

15. The method of claim 14, wherein the refractory particles are based on metal oxides or metals.

16. The method according to claim 1, wherein the deposition of the enamel layer (14) is performed by screen printing using a screen printing screen having a mesh opening of at least 40 μm.

17. The method according to claim 1, wherein: - the method comprises, between step b) and step c), a step b1) of pre-firing the enamel layer (14), during which the stack (12) of thin layers located below the enamel layer (14) is at least partially dissolved by the enamel layer (14), and - In step c), the first glass sheet (10) and the additional glass sheet (20) are bent together with the enamel layer (14) facing the additional glass sheet (20).

18. Method according to claim 1, wherein the additional glass sheet (20) carries a stack (22) of additional thin layers on the face opposite to the face facing the laminating interlayer (30).

19. The method according to claim 18, wherein the stack (22) of additional thin layers is a stack with low emissivity comprising a transparent conductive oxide.

20. A laminated curved glazing unit obtained by the method according to any one of claims 1 to 19, comprising a first glass sheet (10) coated with a stack of thin layers (12) on at least a portion of one of the faces of the first glass sheet (10), the first glass sheet (10) being coated with an enamel layer (14) comprising zinc oxide particles having a volume particle size distribution such that the d90 is at most 5 μm on a portion of its surface, the first glass sheet (10) being laminated with an additional glass sheet (20) via a laminating interlayer (30), the enamel layer (14) facing the laminating interlayer (30).

21. A laminated curved glazing unit according to claim 20 for use in a windscreen or roof of a motor vehicle.