A method for preparing porous adsorption material using gasified fine ash

Through acid treatment and thermal activation treatment combined with the use of alkali and metal salts, the problem of low adsorption performance of gasified fine ash is solved, the preparation of porous adsorption materials with high specific surface area and low ash content is achieved, and the adsorption performance is significantly improved.

CN116351394BActive Publication Date: 2024-10-18CCTEG CLEAN ENERGY CO LTD +1
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202310233743.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-03-13
Publication Date
2024-10-18
Estimated Expiration
2043-03-13

AI Technical Summary

Technical Problem

In the existing technology, the adsorption performance of gasified fine ash is low, and differences in pore distribution and characteristic parameters of activated carbon affect its utilization value, resulting in problems of high ash content and low adsorption performance.

Method used

By subjecting gasified fine ash to acid treatment and thermal activation, combined with the use of alkali and metal salts, a specific preparation process is designed to increase the specific surface area and achieve the preparation of porous adsorbent materials. Specific steps include acid treatment, cleaning, drying, thermal activation treatment and pickling, etc., using alkali and metal salts for multi-point activation under high temperature conditions to generate more reactive ash and increase porosity and specific surface area.

Benefits of technology

The specific surface area of ​​the gasified fine ash-based adsorption material is increased, the ash content is reduced, and the active sites for adsorption are enhanced, resulting in a porous adsorption material with high specific surface area and low ash content, and the adsorption performance is significantly improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116351394B_ABST
    Figure CN116351394B_ABST
Patent Text Reader

Abstract

The present invention relates to a method for preparing a porous adsorbent material using gasified fine ash, the method comprising the following steps: (1) subjecting the gasified fine ash to an acid treatment, followed by washing and drying to obtain an acid-treated material; (2) subjecting an alkali, a metal salt and the acid-treated material obtained in step (1) to a heat activation treatment after mixing, and after cooling, acid washing, washing and drying to obtain a porous adsorbent material. The method provided by the present invention achieves the preparation of an adsorbent material with a high specific surface area by means of a specific design of the preparation process, by using a specific acid treatment and subsequent alkali, metal salt and heat activation treatment, and the specific surface area of ​​the adsorbent material obtained is ≥1546.23m 2 / g.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of solid waste resource utilization, and in particular to a method for preparing a porous adsorption material by utilizing gasified fine ash. Background Art

[0002] At present, entrained-flow coal gasification technology has become the most widely used technology in my country's coal gasification industry due to its advantages of wide adaptability to coal types, high gasification temperature, high gasification efficiency, large production capacity and environmental friendliness. However, the large amount of ash produced by entrained-flow gasification occupies a large amount of land and causes certain pollution to the soil only through landfill treatment, which has attracted people's attention. In particular, the gasification fine ash contains a high amount of residual carbon, and its resource utilization has become a difficult problem to be solved.

[0003] In the prior art, the main ways to utilize gasification fine ash as a resource include blending, preparing building materials, preparing adsorption materials, using it as a soil conditioner, preparing adsorption materials and catalysts, etc.

[0004] CN115672334A discloses using gasification ash as a carrier, introducing active component nickel and using different additives for modification, thereby improving the problem of easy deactivation of a single active component during the catalytic process and having the potential to realize the utilization of all components of the gasification product.

[0005] CN115571890A discloses a method for preparing polyaluminium ferrosilicate flocculant using gasified ash and its application, which has a turbidity removal rate of 93.7%, a chroma removal rate of 36.5%, and a COD removal rate of 71.0% for steel wastewater, and has a good effect of reducing the turbidity, chroma and COD of the wastewater.

[0006] CN115634562A discloses utilizing CaO, MgO, Na2O, K2O, Fe2O3 and the like in coal gangue, fly ash, gasification ash and desulfurized gypsum as active components to react with CO2 to achieve absorption and solidification of CO2, and the absorption amount of CO2 can reach more than 0.30 g / g of material.

[0007] CN114849646A discloses a modified gasification ash activated carbon adsorption material. The collected gasification ash is kneaded with a binder (coal tar, asphalt), and then subjected to granulation, pyrolysis carbonization, oxidation, drying, reduction, calcination and other processes to finally obtain the modified gasification ash activated carbon adsorption material.

[0008] In summary, the disclosed methods for resource utilization of gasification ash indicate that gasification ash has high potential for adsorption utilization value, but there are large differences in the pore distribution and comparative area of ​​gasification fine ash produced by different gasification processes, and the pore characteristic parameters of the fine ash are far from those of activated carbon. This has an adverse effect on the adsorption utilization value of gasification fine ash. Furthermore, due to the high carbon and ash contents in gasification fine ash, the current treatment methods cannot fully develop the adsorption value of gasification fine ash. Summary of the invention

[0009] In view of the problems existing in the prior art, the object of the present invention is to provide a method for preparing a porous adsorption material using gasified fine ash, so as to solve the problem of high ash content and low adsorption performance of gasified fine ash-based adsorption materials in the prior art.

[0010] To achieve this object, the present invention adopts the following technical solutions:

[0011] The present invention provides a method for preparing a porous adsorption material by utilizing gasified fine ash, the method comprising the following steps:

[0012] (1) treating the gasified fine ash with acid, and then washing and drying it to obtain an acid-treated material;

[0013] (2) mixing the alkali, the metal salt and the acid-treated material obtained in step (1), and then subjecting the mixture to thermal activation treatment. After cooling, the mixture is acid-washed, washed and dried to obtain a porous adsorption material.

[0014] The method provided by the present invention realizes the preparation of an adsorption material with a high specific surface area by means of a specific design of the preparation process and by using a combination of a specific acid treatment and subsequent alkali, metal salt and thermal activation treatment.

[0015] In the present invention, the gasified fine ash mainly includes unburned carbon and ash.

[0016] In the present invention, the washing after the acid treatment is performed by water washing or alcohol washing until the pH value of the washing water is 6-7.

[0017] In the present invention, the thermal activation treatment is carried out under a protective atmosphere, and the protective atmosphere can be one or a combination of at least two of carbon dioxide, nitrogen, an inert gas such as helium, neon, argon, etc.

[0018] In the present invention, after the heat activation treatment, an acid solution (such as hydrochloric acid, nitric acid or sulfuric acid, with a mass concentration of 20-80%, when the concentration of hydrochloric acid is too high, concentrated hydrochloric acid can be used, and the same applies to other acids) is used for pickling for 5-60 minutes.

[0019] In the present invention, the washing after the heat activation treatment is to perform water washing or alcohol washing until the pH value of the washing water is 6-7.

[0020] As a preferred technical solution of the present invention, the dry ash content of the gasified fine ash in step (1) is 40-70% by mass, for example, it can be 40%, 41%, 42%, 43%, 44%, 45%, 46%, 47%, 48%, 49%, 50%, 51%, 52%, 53%, 54%, 55%, 56%, 57%, 58%, 59%, 60%, 61%, 62%, 63%, 64%, 65%, 66%, 67%, 68%, 69% or 70%, etc., but is not limited to the listed values, and other values ​​not listed within the range are also applicable.

[0021] Preferably, the moisture content of the gasified fine ash in step (1) is 60-70% by mass, for example, it can be 60%, 60.5%, 61%, 61.5%, 62%, 62.5%, 63%, 63.5%, 64%, 64.5%, 65%, 65.5%, 66%, 66.5%, 67%, 67.5%, 68%, 68.5%, 69%, 69.5% or 70%, etc., but is not limited to the listed values, and other values ​​not listed within the range are also applicable.

[0022] As a preferred technical solution of the present invention, the mass ratio of the acid used in the acid treatment in step (1) to the gasified fine ash dry basis is 1:(1-1.2), for example, it can be 1:1, 1:1.01, 1:1.02, 1:1.03, 1:1.04, 1:1.05, 1:1.06, 1:1.07, 1:1.08, 1:1.09, 1:1.1, 1:1.11, 1:1.12, 1:1.13, 1:1.14, 1:1.15, 1:1.16, 1:1.17, 1:1.18, 1:1.19 or 1:1.2, but is not limited to the listed values, and other values ​​not listed within the range are also applicable.

[0023] As a preferred technical solution of the present invention, the acid used in the acid treatment in step (1) includes one or a combination of at least two of concentrated hydrochloric acid, concentrated nitric acid or concentrated sulfuric acid.

[0024] As a preferred technical solution of the present invention, the temperature of the acid treatment in step (1) is 50-90°C, for example, it can be 50°C, 52°C, 54°C, 56°C, 58°C, 60°C, 62°C, 64°C, 66°C, 68°C, 70°C, 72°C, 74°C, 76°C, 78°C, 80°C, 82°C, 84°C, 86°C, 88°C or 90°C, etc., but is not limited to the listed values, and other values ​​not listed within the range are also applicable.

[0025] Preferably, the time of the acid treatment in step (1) is 2-2.5 h, for example, it can be 2 h, 2.02 h, 2.04 h, 2.06 h, 2.08 h, 2.1 h, 2.12 h, 2.14 h, 2.16 h, 2.18 h, 2.2 h, 2.22 h, 2.24 h, 2.26 h, 2.28 h, 2.3 h, 2.32 h, 23.4 h, 2.36 h, 2.38 h, 2.4 h, 2.42 h, 2.44 h, 2.46 h, 2.48 h or 2.5 h, but is not limited to the listed values, and other values ​​not listed within the range are also applicable.

[0026] As a preferred technical solution of the present invention, the moisture content of the acid-treated material in step (1) is ≤3% by mass percentage, for example, it can be 3%, 2.9%, 2.8%, 2.7%, 2.6%, 2.5%, 2.4%, 2.3%, 2.2%, 2.1%, 2%, 1.9%, 1.8%, 1.7%, 1.6%, 1.5%, 1.4%, 1.3%, 1.2%, 1.1% or 1%, etc., but is not limited to the listed values, and other values ​​not listed within the range are also applicable.

[0027] Preferably, the particle size of the acid-treated material in the mixture in step (2) is ≤0.5 mm.

[0028] In the present invention, the particle size of the mixed medium-acid treated material can be an aggregate of particles of a single particle size within a limited range, or an aggregate of all particles within a certain particle size range, such as an aggregate of particles with a particle size of 0.1 mm, an aggregate of particles with a particle size of 0.01 mm, an aggregate of all particles within a particle size range of 0.2-0.4 mm, an aggregate of all particles within a particle size range of 0.1-0.3 mm, an aggregate of all particles within a particle size range of 0.01-0.4 mm, etc.

[0029] As a preferred technical solution of the present invention, the alkali in step (2) includes one or a combination of at least two of sodium hydroxide, potassium hydroxide or calcium hydroxide.

[0030] Preferably, the metal salt in step (2) comprises copper salt and / or nickel salt.

[0031] In the present invention, the copper salt can be copper sulfate, copper chloride, copper nitrate, basic copper carbonate, etc.

[0032] In the present invention, the nickel salt may be nickel sulfate, nickel chloride, nickel nitrate, basic nickel carbonate, etc.

[0033] As a preferred technical solution of the present invention, the mass ratio of the base to the metal salt in step (2) is 1:(0.05-0.2), for example, it can be 1:0.05, 1:0.055, 1:0.06, 1:0.065, 1:0.07, 1:0.075, 1:0.08, 1:0.085, 1:0.09, 1:0.095, 1:0.1, 1:0.105, 1:0.11, 1:0.115, 1:0. :0.12, 1:0.125, 1:0.13, 1:0.135, 1:0.14, 1:0.145, 1:0.15, 1:0.155, 1:0.16, 1:0.165, 1:0.17, 1:0.175, 1:0.18, 1:0.185, 1:0.19, 1:0.195 or 1:0.2, etc., but not limited to the listed values, other values ​​not listed in the range are also applicable.

[0034] Preferably, the mass ratio of the gasified fine ash dry basis to the mixture consisting of alkali and metal salt in the mixing of step (2) is 1:(3-4), for example, it can be 1:3, 1:3.02, 1:3.04, 1:3.06, 1:3.08, 1:3.1, 1:3.12, 1:3.14, 1:3.16, 1:3.18, 1:3.2, 1:3.22, 1:3.24, 1:3.26, 1:3.28, 1:3.3, 1:3.32, 1:3.34, 1:3.36, 1:3.38, 1:3.4, 1:3.42, 1:3.44, 1:3.46 , 1:3.48, 1:3.5, 1:3.52, 1:3.54, 1:3.56, 1:3.58, 1:3.6, 1:3.62, 1:3.64, 1:3.66, 1:3.68, 1:3.7, 1:3.72, 1:3.74, 1:3.76, 1:3.78, 1:3.8, 1:3.82, 1:3.84, 1:3.86, 1:3.88, 1:3.9, 1:3.92, 1:3.94, 1:3.96, 1:3.98 or 1:4, but are not limited to the listed values, and other values ​​not listed in the range are also applicable.

[0035] As a preferred technical solution of the present invention, the temperature of the thermal activation treatment in step (2) is 850-900°C, for example, it can be 850°C, 852°C, 854°C, 856°C, 858°C, 860°C, 862°C, 864°C, 866°C, 868°C, 870°C, 872°C, 874°C, 876°C, 878°C, 880°C, 882°C, 884°C, 886°C, 888°C, 890°C, 892°C, 894°C, 896°C, 898°C or 900°C, but is not limited to the listed values, and other values ​​not listed within the range are also applicable.

[0036] Preferably, the time of the thermal activation treatment in step (2) is 1-2 h, for example, 1 h, 1.02 h, 1.04 h, 1.06 h, 1.08 h, 1.1 h, 1.12 h, 1.14 h, 1.16 h, 1.18 h, 1.2 h, 1.22 h, 1.24 h, 1.26 h, 1.28 h, 1.3 h, 1.32 h, 1.34 h, 1.36 h, 1.38 h, 1.4 h, 1.42 h, 1.44 h, 1.46 h, 1.48 h, 1. 94h, 1.96h, 1.98h or 2h, but are not limited to the listed values, and other values ​​not listed in the range are also applicable.

[0037] As a preferred technical solution of the present invention, the method comprises the following steps:

[0038] (1) treating the gasified fine ash with acid, and then washing and drying it to obtain an acid-treated material;

[0039] Step (1) The dry ash content of the gasified fine ash is 40-70% by mass percentage; the water content of the gasified fine ash is 60-70% by mass percentage; the mass ratio of the acid used in the acid treatment to the dry basis of the gasified fine ash is 1:(1-1.2); the acid used in the acid treatment includes one or a combination of at least two of concentrated hydrochloric acid, concentrated nitric acid or concentrated sulfuric acid; the temperature of the acid treatment is 50-90°C; the time of the acid treatment is 2-2.5h; the water content of the acid-treated material is ≤3% by mass percentage;

[0040] (2) mixing the alkali, the metal salt and the acid-treated material obtained in step (1), and then subjecting the mixture to thermal activation treatment, and then acid-washing, washing and drying the mixture after cooling to obtain a porous adsorption material;

[0041] The alkali in step (2) comprises one or a combination of at least two of sodium hydroxide, potassium hydroxide or calcium hydroxide; the metal salt comprises copper salt and / or nickel salt; the mass ratio of the alkali to the metal salt is 1:(0.05-0.2); the particle size of the acid-treated material in the mixture is ≤0.5 mm; the mass ratio of the dry basis of the gasified fine ash in the mixture to the mixture consisting of the alkali and the metal salt is 1:(3-4); the temperature of the thermal activation treatment is 850-900° C.; and the time of the thermal activation treatment is 1-2 h.

[0042] Compared with the prior art solutions, the present invention has the following beneficial effects:

[0043] In the present invention, the gasified fine ash is mixed with acid and heated for pre-reaction to improve the efficiency of thermal activation treatment, reduce the influence of unstable ash on the pore expansion effect during the thermal activation treatment, and improve the porosity of the fine ash, increase its specific surface area, react with stable ash to generate more reactive ash, and increase the active points of adsorption through multi-point activation of alkali and metal salt under high temperature conditions. After thermal activation treatment, after further acid washing, the more reactive ash reacts with acid to further reduce ash and expand pores, thereby obtaining a gasified fine ash-based adsorption material with extremely low ash content and high specific surface area. The specific surface area of ​​the obtained adsorption material is ≥1546.23m 2 / g. BRIEF DESCRIPTION OF THE DRAWINGS

[0044] Figure 1 The present invention provides a flowchart of a method for preparing a porous adsorption material by utilizing gasified fine ash.

[0045] The present invention is further described in detail below. However, the following examples are only simplified examples of the present invention and do not represent or limit the scope of protection of the present invention. The scope of protection of the present invention shall be subject to the claims. DETAILED DESCRIPTION

[0046] To better illustrate the present invention and facilitate understanding of the technical solution of the present invention, typical but non-limiting embodiments of the present invention are as follows:

[0047] Depend on Figure 1 It can be seen that after the gasified fine ash is treated with acid, it is pickled, washed and dried to obtain an acid-treated material, which is then mixed with alkali and metal salts and subjected to thermal activation treatment. After the thermal activation treatment, the gasified fine ash-based porous adsorption material is obtained by washing and drying.

[0048] The specific embodiments are as follows:

[0049] Example 1

[0050] This embodiment provides a method for preparing a porous adsorption material by using gasified fine ash, the method comprising the following steps:

[0051] (1) treating the gasified fine ash with acid, and then washing and drying it to obtain an acid-treated material;

[0052] Step (1) The dry ash content of the gasified fine ash is 48.13% by mass percentage; the water content of the gasified fine ash is 66.5% by mass percentage; the mass ratio of the acid used in the acid treatment to the dry basis of the gasified fine ash is 1:1.1; the acid used in the acid treatment is concentrated hydrochloric acid; the temperature of the acid treatment is 50° C.; the time of the acid treatment is 2 hours; the water content of the acid-treated material is 3% by mass percentage;

[0053] (2) mixing the alkali, the metal salt and the acid-treated material obtained in step (1), and subjecting the mixture to thermal activation treatment (in a carbon dioxide atmosphere), and then cooling, acid washing, washing and drying to obtain a porous adsorption material;

[0054] In step (2), the alkali is sodium hydroxide; the metal salt is cupric chloride; the mass ratio of the alkali to the metal salt is 1:0.15; the mixed acid-treated material is an aggregate with a particle size of ≤0.5 mm; the mass ratio of the mixed gasified fine ash dry basis to the mixture composed of the alkali and the metal salt is 1:3; the temperature of the thermal activation treatment is 900° C.; the time of the thermal activation treatment is 2 hours; and the pickling is carried out using hydrochloric acid with a mass concentration of 20% for 50 minutes.

[0055] The performance indicators of the obtained porous adsorption materials are shown in Table 1.

[0056] Example 2

[0057] This embodiment provides a method for preparing a porous adsorption material by using gasified fine ash, the method comprising the following steps:

[0058] (1) treating the gasified fine ash with acid, and then washing and drying it to obtain an acid-treated material;

[0059] Step (1) The dry ash content of the gasified fine ash is 62.04% by mass percentage; the water content of the gasified fine ash is 68.4% by mass percentage; the mass ratio of the acid used in the acid treatment to the dry basis of the gasified fine ash is 1:1.2; the acid used in the acid treatment is concentrated sulfuric acid; the temperature of the acid treatment is 90° C.; the time of the acid treatment is 2.5 hours; the water content of the acid-treated material is 2% by mass percentage;

[0060] (2) mixing the alkali, the metal salt and the acid-treated material obtained in step (1), and subjecting the mixture to thermal activation treatment (in a carbon dioxide atmosphere), and then cooling, acid washing, washing and drying to obtain a porous adsorption material;

[0061] In step (2), the alkali is potassium hydroxide; the metal salt is cupric chloride; the mass ratio of the alkali to the metal salt is 1:0.2; the mixed acid-treated material is an aggregate with a particle size of ≤0.1 mm; the mass ratio of the mixed gasified fine ash dry basis to the mixture composed of the alkali and the metal salt is 1:3.5; the temperature of the thermal activation treatment is 900° C.; the time of the thermal activation treatment is 2 hours; and the pickling is carried out using sulfuric acid with a mass concentration of 80% for 5 minutes.

[0062] The performance indicators of the obtained porous adsorption materials are shown in Table 1.

[0063] Example 3

[0064] This embodiment provides a method for preparing a porous adsorption material by using gasified fine ash, the method comprising the following steps:

[0065] (1) treating the gasified fine ash with acid, and then washing and drying it to obtain an acid-treated material;

[0066] Step (1) The dry ash content of the gasified fine ash is 66.48% by mass percentage; the water content of the gasified fine ash is 65.14% by mass percentage; the mass ratio of the acid used in the acid treatment to the dry basis of the gasified fine ash is 1:1; the acid used in the acid treatment is concentrated sulfuric acid; the temperature of the acid treatment is 80° C.; the time of the acid treatment is 2 hours; the water content of the acid-treated material is 3% by mass percentage;

[0067] (2) mixing the alkali, the metal salt and the acid-treated material obtained in step (1), and subjecting the mixture to thermal activation treatment (argon gas), and then cooling, acid washing, washing and drying to obtain a porous adsorption material;

[0068] The alkali in step (2) is potassium hydroxide; the metal salt includes copper salt and / or nickel salt; the mass ratio of the alkali to the metal salt is 1:0.05; the particle size of the acid-treated material in the mixture is ≤0.075 mm; the mass ratio of the gasified fine ash dry basis to the mixture composed of the alkali and the metal salt in the mixture is 1:4; the temperature of the thermal activation treatment is 850° C.; the time of the thermal activation treatment is 1 hour; and the pickling is carried out for 30 minutes using nitric acid with a mass concentration of 40%.

[0069] The performance indicators of the obtained porous adsorption materials are shown in Table 1.

[0070] Example 4

[0071] This embodiment provides a method for preparing a porous adsorption material by using gasified fine ash, the method comprising the following steps:

[0072] (1) treating the gasified fine ash with acid, and then washing and drying it to obtain an acid-treated material;

[0073] Step (1) The dry ash content of the gasified fine ash is 42.82% by mass percentage; the water content of the gasified fine ash is 64% by mass percentage; the mass ratio of the acid used in the acid treatment to the dry basis of the gasified fine ash is 1:1; the acid used in the acid treatment is concentrated nitric acid; the temperature of the acid treatment is 70° C.; the time of the acid treatment is 2 hours; the water content of the acid-treated material is 1% by mass percentage;

[0074] (2) mixing the alkali, the metal salt and the acid-treated material obtained in step (1), and subjecting the mixture to thermal activation treatment (nitrogen), and then acid-washing, washing and drying the mixture after cooling to obtain a porous adsorption material;

[0075] The alkaline calcium hydroxide of step (2); the metal salt is nickel chloride; the mass ratio of the alkali to the metal salt is 1:0.1; the mixed acid-treated material is an aggregate with a particle size of ≤0.2 mm; the mass ratio of the mixed gasified fine ash dry basis to the mixture composed of the alkali and the metal salt is 1:3; the temperature of the thermal activation treatment is 900° C.; the time of the thermal activation treatment is 1 hour; and the pickling is carried out using nitric acid with a mass concentration of 50% for 30 minutes.

[0076] The performance indicators of the obtained porous adsorption materials are shown in Table 1.

[0077] Example 5

[0078] The only difference from Example 1 is that no acid treatment is performed. That is, the gasified fine ash is washed and dried and then directly proceeds to step (2). The performance indicators of the obtained porous adsorption material are shown in Table 1.

[0079] Example 6

[0080] The only difference from Example 1 is that no alkali and metal salt are used in the thermal activation process. The performance indicators of the obtained porous adsorption material are shown in Table 1.

[0081] Example 7

[0082] The only difference from Example 1 is that no metal salt is used in the thermal activation process. The performance indicators of the obtained porous adsorption material are shown in Table 1.

[0083] Example 8

[0084] The only difference from Example 1 is that after thermal activation, acid washing is not used. The performance indicators of the obtained porous adsorption material are shown in Table 1.

[0085] Table 1

[0086]

[0087]

[0088] The porous adsorption materials obtained in Examples 1-8 were tested for iodine adsorption performance with reference to the national standard GB / T7702.7-2008. The specific results are shown in Table 2 below:

[0089] Table 2

[0090] <![CDATA[Iodine adsorption value / mg·g -1 > Example 1 1597 Example 2 1876 Example 3 1721 Example 4 2120 Example 5 1089 Example 6 525 Example 7 1402 Example 8 894

[0091] It can be seen that the adsorption material provided in the present invention has good adsorption performance, and the adsorption examples are only illustrative examples and are not limited to iodine, and may also be other substances similar to iodine.

[0092] It is stated that the present invention illustrates the detailed structural features of the present invention through the above embodiments, but the present invention is not limited to the above detailed structural features, that is, it does not mean that the present invention must rely on the above detailed structural features to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of the components selected by the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.

[0093] The preferred embodiments of the present invention are described in detail above. However, the present invention is not limited to the specific details in the above embodiments. Within the technical concept of the present invention, a variety of simple modifications can be made to the technical solution of the present invention, and these simple modifications all belong to the protection scope of the present invention.

[0094] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present invention will not further describe various possible combinations.

[0095] In addition, various embodiments of the present invention may be arbitrarily combined, and as long as they do not violate the concept of the present invention, they should also be regarded as the contents disclosed by the present invention.

Claims

1. A method for preparing a porous adsorption material by utilizing gasified fine ash, characterized in that: The method comprises the following steps: (1) treating the gasified fine ash with acid, and then washing and drying it to obtain an acid-treated material; (2) mixing the alkali, the metal salt and the acid-treated material obtained in step (1) and performing a heat activation treatment, cooling, acid washing, washing and drying to obtain a porous adsorption material; The mass ratio of the acid used in the acid treatment of step (1) to the gasified fine ash dry basis is 1:(1-1.2); the acid used in the acid treatment comprises one or a combination of at least two of concentrated hydrochloric acid, concentrated nitric acid or concentrated sulfuric acid; The mass ratio of the alkali to the metal salt in step (2) is 1:(0.05-0.2); the metal salt includes copper salt and / or nickel salt; the mass ratio of the gasified fine ash dry basis to the mixture composed of the alkali and the metal salt in the mixing is 1:(3-4); and the temperature of the thermal activation treatment is 850-900°C.

2. The method according to claim 1, wherein: The dry ash content of the gasified fine ash in step (1) is 40-70% by mass.

3. The method according to claim 1, wherein: The water content of the gasified fine ash in step (1) is 60-70% by mass.

4. The method according to claim 1, wherein: The temperature of the acid treatment in step (1) is 50-90°C.

5. The method according to claim 1, wherein: The time of the acid treatment in step (1) is 2-2.5h.

6. The method according to claim 1, wherein: The moisture content of the acid-treated material in step (1) is ≤3% by mass.

7. The method according to claim 1, wherein: The particle size of the acid-treated material in the mixture in step (2) is ≤0.5 mm.

8. The method according to claim 1, wherein: The alkali in step (2) comprises one or a combination of at least two of sodium hydroxide, potassium hydroxide or calcium hydroxide.

9. The method according to claim 1, wherein: The time of the thermal activation treatment in step (2) is 1-2 hours.

10. The method according to any one of claims 1 to 9, wherein: The method comprises the following steps: (1) treating the gasified fine ash with acid, and then washing and drying it to obtain an acid-treated material; The dry ash content of the gasified fine ash in step (1) is 40-70% by mass; the water content of the gasified fine ash is 60-70% by mass; the mass ratio of the acid used in the acid treatment to the dry basis of the gasified fine ash is 1:(1-1.2); the acid used in the acid treatment comprises one or a combination of at least two of concentrated hydrochloric acid, concentrated nitric acid or concentrated sulfuric acid; the temperature of the acid treatment is 50-90° C.; the time of the acid treatment is 2-2.5 hours; the water content of the acid-treated material is ≤3% by mass; (2) mixing the alkali, the metal salt and the acid-treated material obtained in step (1) and performing a heat activation treatment, cooling, acid washing, washing and drying to obtain a porous adsorption material; The alkali in step (2) comprises one or a combination of at least two of sodium hydroxide, potassium hydroxide or calcium hydroxide; the metal salt comprises copper salt and / or nickel salt; the mass ratio of the alkali to the metal salt is 1:(0.05-0.2); the particle size of the acid-treated material in the mixture is ≤0.5 mm; the mass ratio of the dry basis of the gasified fine ash in the mixture to the mixture consisting of the alkali and the metal salt is 1:(3-4); the temperature of the thermal activation treatment is 850-900° C.; and the time of the thermal activation treatment is 1-2 h.

Citation Information

Patent Citations

  • Multi-grade porous carbon material with ultrahigh specific surface area and preparation method and application of multi-grade porous carbon material

    CN108423678A

  • Preparation of biochar taking coal-fired fly ash as raw material and application of biochar as living bacteria carrier

    CN111099589A