A kind of tetrabromobisphenol A containing flexible group and its preparation method and application

By reacting with cashew glycerol ether, the dust pollution and environmental pollution problems when tetrabromobenzene A are solved when mixing with liquid curing agents, and lower cost use and higher flame retardant are achieved. performance.

CN116354803BActive Publication Date: 2024-11-26SHANDONG TIANYI CHEM
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310230735.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-03-08
Publication Date
2024-11-26
Estimated Expiration
2043-03-08

AI Technical Summary

Technical Problem

Tetrabromobisphenol A cannot be blended directly when mixed with liquid curing agent, resulting in dust pollution and environmental pollution, and requires dilution with organic solvents, increasing costs and hazard risks.

Method used

By reacting with cashew glyceryl ether, tetrabromobenzene A is modified, reducing its viscosity, making it more convenient when mixing with liquid curing agent, avoiding dilution with organic solvents, and using cashew glyceryl ether modified tetrabromobenzene bisphenol modified A. The phenolic hydroxyl group attacks the epoxy group, resulting in the ring opening connection with the phenolic hydroxyl group, forming tetrabromobisphenol A with flexible groups.

Benefits of technology

The viscosity of tetrabromobisphenol A is reduced, making it flowable, easy to blend, reduces the risk of environmental pollution, and improves the mechanical properties of flame retardants, especially in terms of tensile and impact strength.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116354803B_ABST
    Figure CN116354803B_ABST
Patent Text Reader

Abstract

The present invention provides a tetrabromobisphenol A containing a flexible group, a preparation method thereof and an application thereof, which solves the technical problem that the existing tetrabromobisphenol A cannot be directly blended with a liquid curing agent. The tetrabromobisphenol A containing a flexible group has a structure shown in the following formula (I) or formula (II): #imgabs0#, wherein R 1 , R 2 All of them are carbon 15-alkyl side chains of cardanol; the present invention also provides a preparation method and application of tetrabromobisphenol A containing flexible groups, which can be widely used in the field of polymer material technology.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of polymer materials, and in particular to tetrabromobisphenol A containing a flexible group, a preparation method thereof, and an application thereof. Background Art

[0002] Tetrabromobisphenol A is a bromine-containing organic flame retardant with multiple uses. It is both a reactive flame retardant and an additive flame retardant. It is also an important intermediate for synthesizing other flame retardants. It can make materials have excellent flame resistance and self-extinguishing properties. It is widely used in polymer material flame retardants. Due to its good flame retardant properties, its production capacity and market demand are expanding year by year.

[0003] As we all know, tetrabromobisphenol A is a white powder that is soluble in organic solvents such as methanol, ethanol, acetone, and benzene. On October 27, 2017, the World Health Organization's International Agency for Research on Cancer published a preliminary list of carcinogens for reference, and tetrabromobisphenol A is on the list of Class 2A carcinogens. At present, tetrabromobisphenol A cannot be directly blended with liquid curing agents. Organic solvents are usually added for dissolution and dilution. There are two main problems. First, powdered tetrabromobisphenol A is inconvenient to use and easily causes dust pollution. On the other hand, the addition of organic solvents not only increases the cost of using brominated epoxy resins, but also pollutes the environment and increases the risk of environmental damage. This technical problem needs to be solved urgently. Summary of the invention

[0004] The purpose of the present invention is to solve the shortcomings of the above-mentioned technology and provide a tetrabromobisphenol A containing a flexible group, a preparation method thereof and an application thereof. The tetrabromobisphenol A is modified by cardanol glycerol ether to greatly reduce the viscosity of the tetrabromobisphenol A, so that it is convenient to use when mixed with a liquid curing agent, thereby reducing the cost of use and the risk of environmental damage.

[0005] To this end, the present invention provides a tetrabromobisphenol A containing a flexible group, which has a structure shown in the following formula (I) or formula (II):

[0006]

[0007] , wherein R1 and R2 are both pentadecyl side chains of cardanol.

[0008] Preferably, R1 and R2 have a bond-line structure as shown in any one of the following formulas (III), (IV), (V) and (VI):

[0009]

[0010] Preferably, the tetrabromobisphenol A containing a flexible group has a Brookfield viscosity of 10,000 to 100,000 cPs at 25°C.

[0011] A method for preparing any of the above-mentioned tetrabromobisphenol A containing a flexible group, comprising: reacting cardanol glycerol ether and tetrabromobisphenol A under the action of a catalyst to obtain tetrabromobisphenol A containing a flexible group; wherein the tetrabromobisphenol A has a structure shown in the following formula (VII):

[0012]

[0013] Preferably, the catalyst is triphenylphosphine, and its addition amount is 0.05-0.48% of the total mass. The total mass is the sum of the weights of all raw materials added to prepare the tetrabromobisphenol A containing flexible groups by the above-mentioned cardanol and tetrabromobisphenol A under the action of the catalyst.

[0014] Preferably, the raw materials also include an antioxidant, and the amount of the antioxidant added is 0.09-0.11% of the total mass. The total mass is the sum of the weights of all raw materials added to prepare the tetrabromobisphenol A containing flexible groups by the above-mentioned cardanol and tetrabromobisphenol A under the action of a catalyst.

[0015] Preferably, the antioxidant is a mixture of the antioxidant 1010 and the antioxidant 168, and the mass ratio of the antioxidant 1010 to the antioxidant 168 is 2.0 to 2.75:1.

[0016] Preferably, the preparation method of cardanol glycerol ether comprises: stirring cardanol, a quaternary ammonium salt catalyst and an excess of epichlorohydrin under a nitrogen environment and heating to 100°C, reacting for a period of time and then cooling to 55°C, adding sodium hydroxide solution once or multiple times and stirring evenly, reacting for a period of time each time, preferably adding sodium hydroxide solution multiple times to ensure complete cyclization; after completion, adding water to wash while hot to wash away the generated sodium chloride, separating the liquids to obtain the organic phase; then adding water to wash once or multiple times until neutral, separating the liquids to obtain the organic phase; removing the excess epichlorohydrin by distillation under reduced pressure; and obtaining cardanol glycerol ether.

[0017] Preferably, the cardanol glycerol ether is brominated cardanol glycerol ether, and its preparation method comprises: adding cardanol and dichloromethane into a four-necked flask; adding bromine dropwise at 20°C for bromination, keeping warm and stirring for a period of time after the addition, adding sodium sulfite solution for bleaching, separating and taking the lower layer of liquid, and repeating the bleaching; washing with deionized water to obtain brominated cardanol; stirring the obtained brominated cardanol, quaternary ammonium salt catalyst and excess epichlorohydrin under a nitrogen environment and heating to 100°C, reacting for a period of time and then cooling to 55°C, adding sodium hydroxide solution once or multiple times and stirring evenly, reacting for a period of time each time, preferably adding sodium hydroxide solution multiple times to ensure complete cyclization; after completion, adding water to wash while hot to wash off the generated sodium chloride, separating and taking the organic phase; adding water to wash until neutral once or multiple times, separating and taking the organic phase; removing the excess epichlorohydrin by vacuum distillation; obtaining brominated cardanol glycerol ether.

[0018]

[0019] Preferably, the quaternary ammonium salt catalyst is one or both of benzyltriethylammonium chloride and tetrabutylammonium hydrogen sulfate.

[0020] The application of the tetrabromobisphenol A containing a flexible group described in any of the above items is to use one or both of the structures of formula (I) and formula (II) as a polymer flame retardant in flame-retardant epoxy polymer materials.

[0021] The beneficial effects of the present invention are as follows: the present application provides a tetrabromobisphenol A containing a flexible group, a preparation method thereof, and an application thereof. In the preparation method of tetrabromobisphenol A modified with cardanol glycerol ether, a phenolic hydroxyl group attacks the carbon atom of the epoxy group in the cardanol glycerol ether, causing the rupture of the CO bond, opening the epoxy group, and connecting with the phenolic hydroxyl group to obtain tetrabromobisphenol A modified with cardanol glycerol ether. The tetrabromobisphenol A modified with cardanol glycerol ether has the rigidity and flexibility characteristics of cardanol, has a greatly reduced viscosity, and can flow at room temperature, so that it can be conveniently used when mixed with a liquid curing agent, achieving an easy and uniform blending effect, and can be used without the use of an organic solvent diluent, thereby reducing the use cost and the risk of environmental damage.

[0022] The tetrabromobisphenol A containing flexible groups prepared by modifying tetrabromobisphenol A with cardanol glycerol ether improves the mechanical properties of the flame retardant polymer. The tensile and unnotched impact tests show that the tensile and impact strengths are significantly improved compared with brominated epoxy resins. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] In order to more clearly illustrate the technical solutions in the embodiments of the present application, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative labor.

[0024] Figure 1 is the infrared spectrum of brominated cardanol glyceryl ether;

[0025] Figure 2 This is the infrared spectrum of tetrabromobisphenol A containing flexible groups obtained in Example 6;

[0026] Figure 3 This is the infrared spectrum of tetrabromobisphenol A containing flexible groups prepared in Example 9. DETAILED DESCRIPTION

[0027] In order to make the technical problems, technical solutions and beneficial effects to be solved by the present application more clearly understood, the present application is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present application and are not used to limit the present application.

[0028] Unless otherwise specified, the methods used in the present invention are all conventional methods; the raw materials and devices used are all conventional commercially available products unless otherwise specified.

[0029] Example

[0030] Example 1

[0031] Synthesis of cardanol glycerol ether: 140g of epichlorohydrin, 111g of cardanol, and 0.4g of benzyltriethylammonium chloride are added to a four-necked flask, a reflux condenser and a thermometer are installed, nitrogen is passed, and slow heating is started. After 1.5h of stirring, the temperature is raised to 100°C, and the reaction is kept warm for 3h. Excess epichlorohydrin is removed by vacuum distillation; the mixture is transferred to a 65°C water bath, and when the temperature drops to 95°C, 29g of solvent toluene is added, and the temperature drops to about 66°C after stirring for 0.5h. Then, 75g of liquid alkali with a mass fraction of 25% is added dropwise, and the temperature is maintained at 60-65°C for 1.5h. After the addition is completed, the mixture is kept warm and stirred at 56-58°C for 5.5h; during the addition of liquid alkali, solid precipitates appear. After the reaction is completed, the product becomes a brown transparent liquid, which is cardanol glycerol ether.

[0032] After testing, the epoxy equivalent is 582.87 g / mol.

[0033] Example 2

[0034] Synthesis of cardanol glycerol ether: Add 140g of epichlorohydrin, 111g of cardanol, and 0.4g of benzyltriethylammonium chloride into a four-necked flask, install a reflux condenser and a thermometer, pass nitrogen, and start heating slowly. After 1.5h of stirring, heat to 100°C and keep warm for 3h. Transfer to a 55°C water bath, and when the temperature drops to 55°C, add 46.25g of a 30% sodium hydroxide solution by mass, and control the addition time to 0.5-1h. After the addition is completed, react for 0.5h; then add 46.25g of a 30% sodium hydroxide solution by mass again, and control the addition time to 0.5-1h. After the addition is completed, react for 5h; after the end, add 57g of process water to wash and stir for 30min. After standing, take the organic phase, add 65g of process water to wash, and wash until neutral. The organic phase was distilled under reduced pressure at 123° C. and −0.095 MPa to remove excess epichlorohydrin, and finally a yellow transparent liquid was obtained, which was cardanol glycerol ether.

[0035] After testing, the epoxy equivalent is 390.21 g / mol.

[0036] Example 3

[0037] Synthesis of cardanol glycerol ether: 271.6g of epichlorohydrin, 111g of cardanol, and 0.4g of benzyltriethylammonium chloride were added to a four-necked flask, a reflux condenser and a thermometer were installed, nitrogen was passed, and slow heating was started. The entire preparation process is the same as in Example 2, and will not be described here. Finally, a yellow transparent liquid was obtained, which is cardanol glycerol ether.

[0038] After testing, the epoxy equivalent is 357.4g / mol.

[0039] Example 4

[0040] Synthesis of cardanol glycerol ether: 300g of epichlorohydrin, 111g of cardanol, and 0.4g of benzyltriethylammonium chloride were added to a four-necked flask, a reflux condenser and a thermometer were installed, nitrogen was passed, and slow heating was started. The entire preparation process was the same as in Example 2, and will not be repeated here.

[0041] After testing, the epoxy equivalent is 382.87 g / mol.

[0042] It can be seen that the epoxy equivalent of the cardanol glycerol ether synthesized in Examples 2-4 is close to the theoretical value of 358.55, while in Example 1 as a comparative example, the epoxy equivalent of the cardanol glycerol ether synthesized is greatly different from the theoretical value.

[0043] Example 5

[0044] Bromination of cardanol: 132.5g cardanol and 325g dichloromethane were added to a four-necked flask. 143g bromine was added dropwise at 20°C, and the mixture was stirred for 2h after the addition was completed. 110g sodium sulfite solution with a mass fraction of 11% was added for bleaching for 2h, and the lower layer of liquid was separated and bleached repeatedly. 250ml deionized water was used to wash the mixture twice to obtain brominated cardanol.

[0045] After testing, the bromine content of the brominated cardanol obtained was 43.63%.

[0046] Repeat the operation of Example 3 for the brominated cardanol obtained, that is, add 271.6g of epichlorohydrin, 111g of brominated cardanol, and 0.4g of benzyltriethylammonium chloride into a four-necked flask, install a reflux condenser and a thermometer, pass nitrogen, and start heating slowly. The entire preparation process is the same as in Example 3, and will not be repeated here. Finally, dark brominated cardanol glycerol ether is prepared.

[0047] The infrared spectrum of brominated cardanol glycerol ether is as follows Figure 1 As shown. Figure 1 It can be seen that there is no hydroxyl-OH absorption peak of brominated cardanol, indicating that the phenolic hydroxyl groups have been converted into epoxy groups.

[0048] Example 6

[0049] Reaction of cardanol glycerol ether with tetrabromobisphenol A: 33.19 g of tetrabromobisphenol A and 50 g of cardanol glycerol ether obtained in Example 2 were weighed and added into a four-necked flask, placed in a 120° C. oil bath, introduced with nitrogen, added 0.03 g of antioxidant 168 and 0.06 g of antioxidant 1010 at 113° C., added 0.08 g of triphenylphosphine at 120° C., started heating, heated to 180° C., and kept warm for 40 min. After the reaction, a dark brown viscous liquid was obtained, and tetrabromobisphenol A containing flexible groups was obtained.

[0050] The amount of triphenylphosphine added is 0.10% of the total mass. The amount of antioxidant added is 0.11% of the total mass; and the mass ratio of antioxidant 1010 to antioxidant 168 is 2:1.

[0051] The infrared spectrum of tetrabromobisphenol A containing flexible groups is as follows: Figure 2 As shown. Figure 2 As you can see, 3290.8cm -1 The broad peak is the new hydroxyl -OH absorption peak generated by the ring-opening reaction of cardanol glycerol ether and tetrabromobisphenol A; 3009.5cm -1 It is the CC stretching vibration peak of the double bond on the long-chain alkane side chain of cardanol; 2921.5cm -1 、2853.4cm -1 The peaks at 1585.6cm correspond to the stretching vibration absorption peaks of CH on methyl and methylene groups; -1 、1448.2cm -1 The peak is the absorption peak of the vibration of the benzene ring skeleton. The tetrabromobisphenol A containing a flexible group of formula (I) is obtained.

[0052]

[0053] , wherein R1 and R2 are both pentadecyl side chains of cardanol.

[0054] R1 and R2 have a bond-line structure as shown in any one of the following formulas (III), (IV), (V) and (VI):

[0055]

[0056] Example 7

[0057] Weigh 66.37g of tetrabromobisphenol A and 100g of cardanol glycerol ether obtained in Example 3 into a four-necked flask, put it into a 120°C oil bath, pass nitrogen, add 0.05g of antioxidant 168 and 0.11g of antioxidant 1010 at 110°C, add 0.8g of triphenylphosphine at 120°C, start heating, heat to 180°C, and keep warm for 40 minutes. After the end, a dark brown viscous liquid is obtained, and tetrabromobisphenol A containing flexible groups is obtained. After testing, the Brookfield viscosity at 25°C is 10640cPs.

[0058] The amount of triphenylphosphine added is 0.48% of the total mass, the amount of antioxidant added is 0.10% of the total mass, and the mass ratio of antioxidant 1010 to antioxidant 168 is 2.2:1.

[0059] Example 8

[0060] 66.37 g of tetrabromobisphenol A, 0.05 g of antioxidant 168, 0.11 g of antioxidant 1010 and 100 g of cardanol glycerol ether obtained in Example 4 were weighed and added to a four-necked flask, placed in a 120°C oil bath, introduced with nitrogen, stirred for 30 min, added with 0.8 g of triphenylphosphine, and began to heat up to 180°C and kept warm for 40 min. After the end, a yellow viscous liquid was obtained, and tetrabromobisphenol A containing a flexible group was obtained. After testing, the Brookfield viscosity at 25°C was 12580 cPs.

[0061] The amount of triphenylphosphine added is 0.48% of the total mass, the amount of antioxidant added is 0.10% of the total mass, and the mass ratio of antioxidant 1010 to antioxidant 168 is 2.2:1.

[0062] Example 9

[0063] 48.56 g of tetrabromobisphenol A, 0.04 g of antioxidant 168, 0.11 g of antioxidant 1010, and 121.45 g of brominated cardanol glycerol ether in Example 5 were weighed and added to a four-necked flask, placed in a 120° C. oil bath, stirred for 30 min, 0.08 g of triphenylphosphine was added, and the temperature was raised to 180° C. and kept warm for 40 min. A dark viscous liquid was obtained when the temperature was raised to 180° C., and tetrabromobisphenol A containing flexible groups was obtained. The Brookfield viscosity at 25° C. was 75840 cPs.

[0064] The amount of triphenylphosphine added is 0.05% of the total mass, the amount of antioxidant added is 0.09% of the total mass, and the mass ratio of antioxidant 1010 to antioxidant 168 is 2.75:1.

[0065] The infrared spectrum of tetrabromobisphenol A containing flexible groups is as follows: Figure 3 As shown. Figure 3It can be seen that the new hydroxyl -OH absorption peak 3374.3 cm -1 , to obtain tetrabromobisphenol A containing a flexible group of formula (II).

[0066]

[0067] , wherein R1 and R2 are both pentadecyl side chains of cardanol.

[0068] R1 and R2 have a bond-line structure as shown in any one of the following formulas (III), (IV), (V) and (VI):

[0069]

[0070]

[0071] Example 10

[0072] Weigh 410g of epichlorohydrin and 400g of tetrabromobisphenol A into a four-necked flask, install a reflux condenser and a thermometer, start heating, add 1.2g of benzyltriethylammonium chloride, heat and stir to 90°C, react for 2.5h, and remove excess epichlorohydrin by vacuum distillation; transfer to a 55°C water bath, cool to 60°C, add 100g of solvent toluene, stir evenly, evenly add 25% sodium hydroxide solution dropwise within 1h and stir evenly, and react for 5h; then add 300g of solvent toluene for extraction, and add 400g of water for washing while hot to wash away the generated sodium chloride, and separate the liquids; then add 400g of hot water at 60°C for washing twice in a row, and separate the liquids; remove the solvent toluene by vacuum distillation to obtain a brominated epoxy resin.

[0073] Application Examples

[0074] Application Example 1

[0075] (1) Weigh 14.1 g of the flexible group-modified tetrabromobisphenol A prepared in Example 8 and mix it with 102.5 g of epoxy resin E51, then add 4.6 g of flame retardant Sb2O3 and 0.2 g of defoamer B-459, place it in a water bath at 80° C. and heat it for 30 min to obtain an epoxy resin mixed solution for later use;

[0076] (2) Place 61.8 g of curing agent C19 in a water bath at 80° C. and heat for 30 min. Set aside;

[0077] (3) Place the polytetrafluoroethylene mold in a drying oven and preheat to 80°C for use;

[0078] (4) Pour the curing agent C19 heated in a water bath in step (2) into the epoxy resin mixture in step (1), stir thoroughly, and then pour into the polytetrafluoroethylene mold in step (3). Then, place the mold in an oven at 80° C. for 2 hours and then take it out. After curing at room temperature for 4 hours, the cured product in the mold is slowly cooled to room temperature and then demolded to obtain a tensile test specimen and a notched impact test specimen.

[0079] Description: The polytetrafluoroethylene mold is provided with a cavity that matches the shape and size of the tensile test specimen and the unnotched impact test specimen.

[0080] 1. Tensile test

[0081] Test standard for tensile test: "Determination of Tensile Properties of Plastics" (GB / T 2567-2021).

[0082] Sample size: Prepare according to GB / T 2567-2021. The sample needs to be made into a dumbbell shape.

[0083] Test method: Clamp the sample so that the long axis of the sample is consistent with the tensile direction of the center line of the upper and lower clamps, continuously load at a certain speed until it is broken, and read the breaking load value. The loading speed is 2mm / min, and each group of samples is not less than 5. If the breaking point of the sample is not in the middle parallel part, the sample is invalid. The average value of all test data is the final test result. The final test results are shown in Table 1 below:

[0084] Table 1: Tensile test results of Application Example 1

[0085]

[0086] 2. Unnotched impact test

[0087] Test standard for unnotched impact test: GB / T 1043.1-2008 "Determination of impact properties of simply supported plastic beams".

[0088] Sample specifications: length (80±2) mm, width (10±0.2) mm, thickness (4±0.2) mm, and span 60 mm.

[0089] Test method: Place the test piece symmetrically and vertically against the support, with the pendulum impact speed at 2.9m / s, release the pendulum steadily, and read the energy absorbed by the impact test. Each group of samples should be no less than 5. The average value of all test data is the final test result. The final test results are shown in Table 2 below:

[0090] Table 2: Unnotched impact test results of Application Example 1

[0091] Num Maximum angle / ° Impact strength / J <![CDATA[Impact strength / KJ / m 2 > average value 134.84 0.412 11.36

[0092] Application Example 2

[0093] (1) Weigh 25 g of the brominated epoxy resin prepared in Example 10 and mix with 100 g of epoxy resin E51, then add 5 g of flame retardant Sb2O3 and 0.2 g of defoamer B-459, place in a water bath at 80°C and heat for 30 min to obtain an epoxy resin mixed solution for later use;

[0094] (2) Place 50 g of curing agent C19 in a water bath at 80°C and heat for 30 min for later use;

[0095] (3) Place the polytetrafluoroethylene mold in a drying oven and preheat to 80°C for use;

[0096] (4) Pour the curing agent C19 heated in a water bath in step (2) into the epoxy resin mixture in step (1), stir thoroughly, and then pour into the polytetrafluoroethylene mold in step (3). Then, place the mold in an oven at 80° C. for 2 hours and then take it out. After curing at room temperature for 4 hours, the cured product in the mold is slowly cooled to room temperature and then demolded to obtain a tensile test specimen and a notched impact test specimen.

[0097] 1. Tensile test

[0098] Test standard for tensile test: "Determination of Tensile Properties of Plastics" (GB / T 2567-2021).

[0099] Sample size: Prepare according to GB / T 2567-2021. The sample needs to be made into a dumbbell shape.

[0100] Test method: Clamp the sample so that the long axis of the sample is consistent with the tensile direction of the center line of the upper and lower clamps, continuously load at a certain speed until failure, and read the failure load value. The loading speed is 2mm / min, and each group of samples is not less than 5. If the fracture point of the sample is not in the middle parallel part, the sample is invalid. The average value of all test data is the final test result. The test results are shown in Table 3 below:

[0101] Table 3: Tensile test results of Application Example 2

[0102]

[0103] 2. Unnotched impact test

[0104] Test standard for unnotched impact test: GB / T 1043.1-2008 "Determination of impact properties of simply supported plastic beams".

[0105] Sample specifications: length (80±2) mm, width (10±0.2) mm, thickness (4±0.2) mm, and span 60 mm.

[0106] Test method: Place the test piece symmetrically and vertically on the support, with the pendulum impact speed at 2.9m / s, release the pendulum steadily, and read the energy absorbed by the impact test. Each group of samples should be no less than 5. The average value of all test data is the final test result. See Table 4 below for the test results:

[0107] Table 4: Unnotched impact test results of Application Example 2

[0108]

[0109]

[0110] Table 5: Tensile test results of application examples 1-2

[0111] Application Examples Tensile strength / MPa Elongation at break / % Application Example 1 29.78 4.40 Application Example 2 26.75 4.67

[0112] Table 6: Unnotched impact test results of application examples 1-2

[0113] Application Examples <![CDATA[Impact strength / KJ / m 2 > Application Example 1 11.36 Application Example 2 8.12

[0114] It can be seen from the test data in Tables 5 and 6 above that the tensile strength and impact strength of tetrabromobisphenol A modified with cardanol glycerol ether are significantly improved. Compared with the brominated epoxy resin flame retardant system, the tensile strength of tetrabromobisphenol A modified with flexible groups is increased by 11.3%, and the impact strength is increased by 39.85%, and the mechanical properties of the flame retardant resin are greatly improved.

[0115] The present invention provides tetrabromobisphenol A containing a flexible group, a preparation method thereof and an application thereof. In the preparation method of tetrabromobisphenol A modified with cardanol glycerol ether, a phenolic hydroxyl group attacks the carbon atom of an epoxy group in cardanol glycerol ether, causing the rupture of a CO bond, opening the epoxy group, and connecting with the phenolic hydroxyl group to obtain tetrabromobisphenol A modified with cardanol glycerol ether. The tetrabromobisphenol A modified with cardanol glycerol ether has the rigidity and flexibility characteristics of cardanol, has a greatly reduced viscosity, and can flow at a room temperature of 25 degrees, so that it can be conveniently used when mixed with a liquid curing agent, achieving an easy and uniform blending effect, and can be used without using an organic solvent diluent, thereby reducing the use cost and the risk of environmental damage.

[0116] The tetrabromobisphenol A containing flexible groups prepared by modifying tetrabromobisphenol A with cardanol glycerol ether improves the mechanical properties of the flame retardant polymer. The tensile and unnotched impact tests show that the tensile and impact strengths are significantly improved compared with brominated epoxy resins.

[0117] It should be noted that:

[0118] (1) Cardanol glycerol ether is prepared, including brominated cardanol glycerol ether, using a quaternary ammonium salt catalyst, preferably benzyl triethyl ammonium chloride used in the embodiment of the present invention, and other quaternary ammonium salt catalysts can also be used. In the actual production process, the quaternary ammonium salt catalyst is usually one or two of benzyl triethyl ammonium chloride and tetrabutyl ammonium hydrogen sulfate.

[0119] (2) The tetrabromobisphenol A containing flexible groups obtained in Examples 7-9 have Brookfield viscosities of 10640 cPs, 12580 cPs, and 75840 cPs at 25°C, respectively; preferably, the tetrabromobisphenol A containing flexible groups of the present invention has a Brookfield viscosity of 10000 to 100000 cPs at 25°C.

[0120] The above description is only a preferred embodiment of the present application and is not intended to limit the present application. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present application should be included in the protection scope of the present application.

Claims

1. A tetrabromobisphenol A containing a flexible group, characterized in that: It has a structure shown in the following formula (I) or formula (II): (I) or (II) Wherein, R1 and R2 are both carbon 15-alkyl side chains of cardanol; The R1 and R2 have a bond-line structure as shown in any one of the following formulas (III), (IV), (V), and (VI): (III) (IV) (V) (WE).

2. A method for preparing a tetrabromobisphenol A containing a flexible group as claimed in claim 1, characterized in that: It includes: Cardanol glycerol ether and tetrabromobisphenol A are reacted under the action of a catalyst to obtain the tetrabromobisphenol A containing a flexible group; wherein the tetrabromobisphenol A has a structure shown in the following formula (VII): (VII).

3. A method for preparing a tetrabromobisphenol A containing a flexible group as claimed in claim 2, characterized in that: The catalyst is triphenylphosphine, and the added amount thereof is 0.05-0.48% of the total mass.

4. A method for preparing a tetrabromobisphenol A containing a flexible group as claimed in claim 3, characterized in that: The raw materials also include antioxidants, the added amount of which is 0.09-0.11% of the total mass.

5. A method for preparing a tetrabromobisphenol A containing a flexible group as claimed in claim 4, characterized in that: The antioxidant is a mixture of the antioxidant 1010 and the antioxidant 168, and the mass ratio of the antioxidant 1010 to the antioxidant 168 is 2.0-2.75:

1.

6. A method for preparing a tetrabromobisphenol A containing a flexible group as claimed in claim 2, characterized in that: The preparation method of the cardanol glycerol ether comprises: stirring cardanol, a quaternary ammonium salt catalyst and an excess of epichlorohydrin in a nitrogen environment and heating to 100°C, reacting for a period of time and then cooling to 55°C, adding a sodium hydroxide solution once or multiple times and stirring evenly, and reacting for a period of time each time; after the reaction, adding water to wash while hot to wash away the generated sodium chloride, separating the liquids to obtain an organic phase; adding water to wash once or multiple times until neutral, separating the liquids to obtain an organic phase; removing the excess epichlorohydrin by distillation under reduced pressure; and obtaining the cardanol glycerol ether.

7. A method for preparing a tetrabromobisphenol A containing a flexible group as claimed in claim 2, characterized in that: The cardanol glycerol ether is brominated cardanol glycerol ether, and its preparation method comprises: adding cardanol and dichloromethane into a four-necked flask; adding bromine dropwise at 20°C for bromination, keeping warm and stirring for a period of time after the adding, adding sodium sulfite solution for bleaching, separating and taking the lower layer of liquid, and repeating the bleaching; washing with deionized water to obtain brominated cardanol; stirring the obtained brominated cardanol, quaternary ammonium salt catalyst and excess epichlorohydrin under a nitrogen environment and heating to 100°C, reacting for a period of time and then cooling to 55°C, adding sodium hydroxide solution once or multiple times and stirring evenly, and reacting for a period of time each time; after the end, adding water to wash while hot to wash away the generated sodium chloride, separating and taking the organic phase; adding water to wash until neutral once or multiple times, separating and taking the organic phase; removing the excess epichlorohydrin by reduced pressure distillation; and obtaining the brominated cardanol glycerol ether.

8. A method for preparing a tetrabromobisphenol A containing a flexible group as claimed in claim 6 or 7, characterized in that: The quaternary ammonium salt catalyst is one or two of benzyltriethylammonium chloride and tetrabutylammonium hydrogen sulfate.

9. The use of tetrabromobisphenol A containing a flexible group according to claim 1, characterized in that: One or both of the structures of formula (I) and formula (II) are used as polymer flame retardants in flame retardant epoxy polymer materials.