A degradable flame-retardant and wear-resistant composite foam material and preparation method thereof

By adding polyvinyl alcohol/oxidized expandable graphene/LDHs composite flame retardant to EVA foam, the thermal expansion of oxidized expandable graphene and the endothermic properties of LDHs are utilized, combined with the cross-linking of guanidine phosphate urea and beet phosphate. The intercalation reaction of alkali solves the problems of flammability and poor wear resistance of EVA materials, achieves excellent flame retardancy, wear resistance and high mechanical properties of the material, and expands its application scope.

CN116355308BActive Publication Date: 2024-10-25FUZHOU UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310430069.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-04-21
Publication Date
2024-10-25
Estimated Expiration
2043-04-21

AI Technical Summary

Technical Problem

EVA foam materials are flammable and have poor wear resistance after foaming, which limits their application in shoe materials that require high wear resistance.

Method used

By adding polyvinyl alcohol/oxidized expandable graphene/LDHs composite flame retardant, the thermal expansion characteristics of oxidized expandable graphene and the endothermic effect of LDHs are utilized, combined with the cross-linking effect of guanidinourea phosphate and the intercalation of betaine phosphate. layer reaction to improve the flame retardant and wear resistance of the material.

Benefits of technology

It achieves the excellent flame retardant, wear-resistant and high mechanical properties of EVA composite foam materials, reduces the material density and wear, and expands its application prospects and socio-economic benefits in the field of shoe materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116355308B_ABST
    Figure CN116355308B_ABST
Patent Text Reader

Abstract

The present invention discloses a degradable flame-retardant and wear-resistant composite foam material and a preparation method thereof. The polyvinyl alcohol / oxidized expandable graphene / LDHs composite flame retardant prepared by the present invention has a scientific and reasonable formula, a simple and practical process flow, and uses polyvinyl alcohol to chemically graft oxidized expandable graphene to significantly improve the compatibility of inorganic additives with EVA polymers. At the same time, a cross-linking reaction occurs with guanidinium urea phosphate under acidic conditions. In addition, the interlayer nitrate and phosphate intercalation of the LDHs composite flame retardant further improves the flame retardant effect, thereby achieving a small amount of addition and easy dispersion. The polyvinyl alcohol / oxidized expandable graphene / LDHs composite flame retardant material has excellent mechanics, wear resistance and anti-skid properties, and has good degradability. At the same time, it also provides new ideas and explorations for the development of new composite additives in the future, and has huge social and economic benefits in practical applications.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of polymer composite foam materials, and in particular relates to a degradable flame-retardant and wear-resistant composite foam material and a preparation method thereof. Background Art

[0002] EVA foam composite materials are widely used in the fields of footwear, construction, packaging, etc. due to their advantages such as low density, strong cushioning and shock absorption ability, and low temperature resistance. Since EVA materials are extremely flammable and have reduced wear resistance after foaming, like most polymer plastics. Such high wear will seriously restrict its application in some footwear materials with high wear resistance requirements. Due to the effect of wear, product failure may occur in severe cases. Therefore, the research of wear-resistant and flame-retardant, degradable EVA composite foam materials has important application value in the field of footwear.

[0003] Layered double hydroxides, also known as LDHs, are inorganic materials with a layered structure (containing a large amount of hydroxyl groups and bound water). They have a strong endothermic effect and can effectively absorb the heat during combustion or intercalate with anions.

[0004] Graphene is a two-dimensional carbonaceous material made of carbon atoms tightly stacked in a hexagonal honeycomb on the same plane. Graphene's novel structure and excellent electrical, thermal, mechanical, and optical properties have attracted the attention of researchers since its discovery. Expandable graphite also has the property of thermal expansion, so it is often used in flame retardants. Oxidized expandable graphene not only has a large number of oxygen-containing functional groups that can eliminate a large number of free radicals in the polymer, but also has the effect of thermal expansion. Summary of the invention

[0005] The purpose of the present invention is to provide a degradable flame-retardant and wear-resistant composite foam material and a preparation method thereof. The present invention has a scientific and reasonable formula, a simple and practical process flow, and aims at the fact that EVA has a very small density, is extremely flammable, and has poor wear resistance and anti-skid performance. By adding polyvinyl alcohol / oxidized expandable graphene / LDHs composite materials, the produced EVA composite foam material has excellent flame retardancy and good wear resistance, has great application prospects, and generates huge social and economic benefits.

[0006] To achieve the above object, the present invention is achieved through the following technical solutions:

[0007] A degradable flame-retardant and wear-resistant composite foam material, whose raw material composition comprises, by weight: 75-95 parts of ethylene-vinyl acetate copolymer, 5-25 parts of polyvinyl alcohol / oxidized expandable graphene / LDHs composite flame retardant, 2.5-3 parts of foaming agent AC, 0.2-1 part of crosslinking agent DCP, and 1-2 parts of stearic acid+zinc stearate+zinc oxide.

[0008] Furthermore, the content of vinyl acetate in the ethylene-vinyl acetate copolymer is 13wt%-20wt%.

[0009] Furthermore, the polyvinyl alcohol / oxidized expandable graphene / LDHs composite flame retardant is prepared by a coprecipitation method, and the specific preparation method comprises the following steps:

[0010] 1) Preparation of oxidized expandable graphene: 3 g of expandable graphite was added to 150 ml of concentrated sulfuric acid, stirred at room temperature for 1 h under high-speed magnetic stirring, and then 5 g of potassium permanganate was slowly added, reacted for 2 h, heated to 90°C, and 150 ml of deionized water and 50 ml of 30 wt.% hydrogen peroxide solution were added respectively, and finally centrifuged several times in a centrifuge at 8000 rpm, washed, and dried to obtain oxidized expandable graphene;

[0011] 2) Preparation of LDHs composite flame retardant: Magnesium nitrate hexahydrate and aluminum nitrate nonahydrate were added into a three-necked flask at a molar ratio of 3:1, and then deionized water was added to dissolve. The three-necked flask was placed in a water bath and heated to 80°C, and stirred continuously. Betaine phosphate was then added, and stirring continued for 3 hours. The mixture was filtered, dried, and ground for later use.

[0012] 3) Preparation of polyvinyl alcohol / oxidized expandable graphene composite flame retardant: 1 g of polyvinyl alcohol, 200 mg of guanidine urea phosphate, 2 ml of 10 wt.% HCl solution and 500 mg of oxidized expandable graphene were dissolved in 200 ml of deionized water, heated to 80°C, mixed for 3 h, centrifuged several times, dried and crushed for later use;

[0013] 4) Preparation of polyvinyl alcohol / oxidized expandable graphene / LDHs composite flame retardant: 5 g of polyvinyl alcohol / oxidized expandable graphene composite flame retardant was ultrasonically dispersed in deionized water, and then 3 g of LDHs composite flame retardant was added. The mixture was stirred continuously, and when a flocculent precipitate was produced, it was quickly filtered and dried for later use.

[0014] Furthermore, the molar ratio of betaine phosphate to the sum of magnesium nitrate hexahydrate and aluminum nitrate nonahydrate is 1:1.

[0015] The method for preparing the degradable flame-retardant and wear-resistant composite foam material comprises the following steps:

[0016] 1) Ethylene-vinyl acetate copolymer, polyvinyl alcohol / oxidized expandable graphene / LDHs composite flame retardant, stearic acid, crosslinking agent DCP and foaming agent AC were mixed evenly and placed in a preheated internal mixer at a heating temperature of 110-120°C and a speed of 20 rpm for 5 minutes;

[0017] 2) The mixture obtained in step 1) is quickly transferred to an open mill and mixed for 10-20 minutes, and then the material is pressed into 3-5 mm thin sheets;

[0018] 3) placing the sheet obtained in step 2) in a preheated flat vulcanizing machine cavity, performing compression molding and foaming at 12 MPa and 175° C. for 300 seconds, and then performing secondary oil pressure molding at 12 MPa and 175° C. for 300 seconds, and water cooling for 400 seconds to obtain a biodegradable flame retardant and wear-resistant composite foam material.

[0019] The present invention adopts polyvinyl alcohol / oxidized expandable graphene / LDHs composite flame retardant as a flame retardant to prepare an EVA composite foam material having the following characteristics: 1) polyvinyl alcohol is degradable, rich in hydroxyl groups, and has good compatibility with EVA polymers, and reacts with oxygen-containing functional groups such as carboxyl groups and epoxy groups rich in the surface of oxidized expandable graphene, thereby improving the compatibility of oxidized expandable graphene with EVA polymers; 2) guanidine urea phosphate can be cross-linked with polyvinyl alcohol under acidic conditions, and amino groups and hydroxyl groups undergo cross-linking reactions, thereby improving the mechanical strength of polyvinyl alcohol as an additive, and at the same time, a large number of benzene rings exist in the structural formula of oxidized expandable graphene, so it can be used as a filler in EVA polymers. The material can improve both rigidity and flexibility at the same time; 3) Oxidized expandable graphene can achieve the effect of blocking flames through its own expansion characteristics during combustion; 4) Since the surface of oxidized expandable graphene is rich in oxygen-containing functional groups, it has a strong negative potential and can electrostatically adsorb with layered double metal hydroxides, thereby improving the dispersibility of LDHs in the polymer matrix; 5) After thermal decomposition, betaine phosphate produces ammonium hydroxide, phosphate and nitrate intercalated LDHs, which significantly increases the interlayer spacing of LDHs. Phosphate and nitrate are intercalated into the interlayer of LDHs during the chemical synthesis process, and the morphology is a hexagonal structure. The interlayer spacing is significantly increased to 0.67nm, which improves the flame retardant performance. Betaine phosphate introduces nitrate and phosphate intercalation into the interlayer of LDHs composite flame retardant, and releases a large amount of acidic gas during combustion, which significantly improves the flame retardant performance of the polymer. In existing EVA foam materials, the reinforcement and flame retardant treatment are mostly based on talcum powder and calcium powder, and a large amount of addition can achieve a certain effect. Polyvinyl alcohol / oxidized expandable graphene / LDHs composite flame retardant is used as an additive to EVA composite foam materials. With a small addition amount, EVA composite foam materials with flame retardant, anti-slip, wear resistance and high mechanical properties are successfully prepared. At the same time, it also provides new ideas and explorations for the development of new flame retardant and degradable materials in the future, and has huge social and economic benefits in practical applications.

[0020] The beneficial effects of the present invention are as follows: the polyvinyl alcohol / oxidized expandable graphene / LDHs composite flame retardant material prepared by the present invention and its application in EVA composite foaming material have scientific and reasonable formula, simple and practical process flow, and prepare polyvinyl alcohol / oxidized expandable graphene / LDHs composite flame retardant composite material in a green and environmentally friendly manner. The present invention utilizes the alcohol hydroxyl group of polyvinyl alcohol and the surface carboxyl group, epoxy group and other oxygen-containing functional groups of oxidized expandable graphene to form an inorganic@organic combination of oxidized expandable graphene and polyvinyl alcohol through chemical bonds and, and due to the cross-linking effect of guanidine urea phosphate on polyvinyl alcohol, the additive has both rigidity and flexibility, and then the LDHs composite flame retardant is electrostatically adsorbed to improve the compatibility of LDHs inorganic composite flame retardant in EVA polymer. The synthesis of LDHs is controlled by phosphobetaine, so that nitrate and phosphate ions are intercalated between LDHs layers, and nitrate and phosphate ions can release acidic gases during the combustion process to achieve a flame retardant effect, further improving the flame retardant effect of the LDHs composite flame retardant. Polyvinyl alcohol / oxidized expandable graphene / LDHs composite flame retardant is used as a flame retardant additive for EVA foaming materials. The amount of addition is small, the compatibility with the EVA matrix is ​​good, it is easy to disperse, and it has a degradable and recyclable effect, and has excellent mechanical, wear-resistant and anti-slip properties. EVA composite foam material has the advantages of light weight, low density, uniform foaming pore size, and good elasticity. At the same time, it also provides new ideas and explorations for the development of new degradable and recyclable materials in the future, and has huge social and economic benefits in practical applications. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 The molecular structure diagram of polyvinyl alcohol / oxidized expandable graphene / LDHs composite flame retardant;

[0022] Figure 2 is the XRD pattern of LDHs composite flame retardant;

[0023] Figure 3 This is the FTIR image of LDHs composite flame retardant;

[0024] Figure 4 This is the SEM image of polyvinyl alcohol / oxidized expandable graphene / LDHs composite flame retardant. DETAILED DESCRIPTION

[0025] The present invention is further described below in conjunction with specific embodiments, but the present invention is not limited to these embodiments.

[0026] The preparation method of polyvinyl alcohol / oxidized expandable graphene / LDHs composite flame retardant comprises the following specific steps:

[0027] 1) Preparation of oxidized expandable graphene: 3 g of expandable graphite was added to 150 ml of concentrated sulfuric acid, stirred at room temperature for 1 h under high-speed magnetic stirring conditions, and then 5 g of potassium permanganate was slowly added. The reaction was continued for 2 h, and the temperature was raised to 90°C. 150 ml of deionized water and 50 ml of 30 wt.% hydrogen peroxide solution were added respectively. Finally, the mixture was centrifuged several times in a centrifuge at 8000 rpm, and a few layers of oxidized expandable graphene were removed. The oxidized expandable graphene was washed and dried to obtain the oxidized expandable graphene.

[0028] 2) Preparation of LDHs composite flame retardant: Add magnesium nitrate hexahydrate and aluminum nitrate nonahydrate in a molar ratio of 3:1 into a three-necked flask, and then add deionized water to dissolve. Place the three-necked flask in a water bath and heat to 80°C, stirring continuously. Then add betaine phosphate (the ratio of betaine phosphate to the sum of the molar amounts of magnesium nitrate hexahydrate and aluminum nitrate nonahydrate is 1:1) and continue stirring for 3 hours, filter, dry and grind for later use.

[0029] 3) Preparation of polyvinyl alcohol / oxidized expandable graphene composite flame retardant: 1 g of polyvinyl alcohol, 200 mg of guanidine urea phosphate, 2 ml of 10 wt.% HCl solution and 500 mg of oxidized expandable graphene were dissolved in 200 ml of deionized water respectively, heated to 80°C, and mixed for 3 hours. After multiple centrifugation, the mixture was dried and crushed for later use.

[0030] 4) Preparation of polyvinyl alcohol / oxidized expandable graphene / LDHs composite flame retardant: 5 g of polyvinyl alcohol / oxidized expandable graphene composite flame retardant was ultrasonically dispersed in deionized water, and 3 g of LDHs composite flame retardant was added and stirred continuously. When flocculent precipitate was produced, it was quickly filtered and dried for use.

[0031] Example 1

[0032] A method for preparing a degradable flame-retardant and wear-resistant composite foam material comprises the following steps:

[0033] 1) 95 parts by weight of EVA, 5 parts by weight of polyvinyl alcohol / oxidized expandable graphene / LDHs composite flame retardant, 0.4 parts by weight of stearic acid, 0.5 parts by weight of zinc stearate, 0.7 parts by weight of zinc oxide, 0.2 parts by weight of dicumyl peroxide and 2.5 parts by weight of AC were mixed and placed in a preheated internal mixer, and the mixture was heated to 110° C. and kneaded at 20 rpm for 5 minutes;

[0034] 2) The mixture obtained in step 1) was quickly transferred to an open mill and mixed for 15 minutes, and then the material was pressed into 4 mm thin sheets;

[0035] 3) placing the sheet obtained in step 2) in a preheated flat vulcanizing machine cavity, performing compression molding and foaming at 12 MPa and 175° C. for 300 seconds, and then performing secondary oil pressure molding at 12 MPa and 175° C. for 300 seconds, and water cooling for 400 seconds to obtain a biodegradable flame retardant and wear-resistant composite foam material.

[0036] Example 2

[0037] A method for preparing a degradable flame-retardant and wear-resistant composite foam material comprises the following steps:

[0038] 1) 90 parts by weight of EVA, 10 parts by weight of polyvinyl alcohol / oxidized expandable graphene / LDHs composite flame retardant, 0.4 parts by weight of stearic acid, 0.5 parts by weight of zinc stearate, 0.7 parts by weight of zinc oxide, 0.2 parts by weight of dicumyl peroxide and 2.5 parts by weight of AC were mixed and placed in a preheated internal mixer, and the mixture was heated to 110° C. and kneaded at 20 rpm for 5 minutes;

[0039] 2) The mixture obtained in step 1) was quickly transferred to an open mill and mixed for 15 minutes, and then the material was pressed into 4 mm thin sheets;

[0040] 3) placing the sheet obtained in step 2) in a preheated flat vulcanizing machine cavity, performing compression molding and foaming at 12 MPa and 175° C. for 300 seconds, and then performing secondary oil pressure molding at 12 MPa and 175° C. for 300 seconds, and water cooling for 400 seconds to obtain a biodegradable flame retardant and wear-resistant composite foam material.

[0041] Example 3

[0042] A method for preparing a degradable flame-retardant and wear-resistant composite foam material comprises the following steps:

[0043] 1) 85 parts by weight of EVA, 15 parts by weight of polyvinyl alcohol / oxidized expandable graphene / LDHs composite flame retardant, 0.4 parts by weight of stearic acid, 0.5 parts by weight of zinc stearate, 0.7 parts by weight of zinc oxide, 0.2 parts by weight of dicumyl peroxide and 2.5 parts by weight of AC were mixed and placed in a preheated internal mixer, and the mixture was heated to 110° C. and kneaded at 20 rpm for 5 minutes;

[0044] 2) The mixture obtained in step 1) was quickly transferred to an open mill and mixed for 15 minutes, and then the material was pressed into 4 mm thin sheets;

[0045] 3) placing the sheet obtained in step 2) in a preheated flat vulcanizing machine cavity, performing compression molding and foaming at 12 MPa and 175° C. for 300 seconds, and then performing secondary oil pressure molding at 12 MPa and 175° C. for 300 seconds, and water cooling for 400 seconds to obtain a biodegradable flame retardant and wear-resistant composite foam material.

[0046] Example 4

[0047] A method for preparing a degradable flame-retardant and wear-resistant composite foam material comprises the following steps:

[0048] 1) 80 parts by weight of EVA, 20 parts by weight of polyvinyl alcohol / oxidized expandable graphene / LDHs composite flame retardant, 0.4 parts by weight of stearic acid, 0.5 parts by weight of zinc stearate, 0.7 parts by weight of zinc oxide, 0.2 parts by weight of dicumyl peroxide and 2.5 parts by weight of AC were mixed and placed in a preheated internal mixer, and the mixture was heated to 110°C and kneaded at 20 rpm for 5 minutes;

[0049] 2) The mixture obtained in step 1) was quickly transferred to an open mill and mixed for 15 minutes, and then the material was pressed into 4 mm thin sheets;

[0050] 3) placing the sheet obtained in step 2) in a preheated flat vulcanizing machine cavity, performing compression molding and foaming at 12 MPa and 175° C. for 300 seconds, and then performing secondary oil pressure molding at 12 MPa and 175° C. for 300 seconds, and water cooling for 400 seconds to obtain a biodegradable flame retardant and wear-resistant composite foam material.

[0051] Example 5

[0052] A method for preparing a degradable flame-retardant and wear-resistant composite foam material comprises the following steps:

[0053] 1) 75 parts by weight of EVA, 25 parts by weight of polyvinyl alcohol / oxidized expandable graphene / LDHs composite flame retardant, 0.4 parts by weight of stearic acid, 0.5 parts by weight of zinc stearate, 0.7 parts by weight of zinc oxide, 0.2 parts by weight of dicumyl peroxide and 2.5 parts by weight of AC were mixed and placed in a preheated internal mixer, and the mixture was heated to 110°C and kneaded at 20 rpm for 5 minutes;

[0054] 2) The mixture obtained in step 1) was quickly transferred to an open mill and mixed for 15 minutes, and then the material was pressed into 4 mm thin sheets;

[0055] 3) placing the sheet obtained in step 2) in a preheated flat vulcanizing machine cavity, performing compression molding and foaming at 12 MPa and 175° C. for 300 seconds, and then performing secondary oil pressure molding at 12 MPa and 175° C. for 300 seconds, and water cooling for 400 seconds to obtain a biodegradable flame retardant and wear-resistant composite foam material.

[0056] Comparative Example 1

[0057] A method for preparing an EVA foam composite material specifically comprises the following steps:

[0058] 1) 85 parts by weight of EVA, 10 parts by weight of unmodified polyvinyl alcohol, 5 parts by weight of unmodified graphene oxide, 0.4 parts by weight of stearic acid, 0.5 parts by weight of zinc stearate, 0.7 parts by weight of zinc oxide, 0.2 parts by weight of dicumyl peroxide and 2.5 parts by weight of AC were mixed and placed in a preheated extruder, and the temperature of each zone was 110° C. and the speed was 20 rpm for extrusion and mixing for 5 minutes;

[0059] 2) The mixture obtained in step 1) was quickly transferred to an open mill and mixed for 15 minutes, and then the material was pressed into 4 mm thin sheets;

[0060] 3) The sheet obtained in step 2) (the mass of the sheet is 1.2 times the volume of the mold in g / ml) is placed in the preheated flat vulcanizer cavity, and is molded and foamed at 12 MPa and 175°C for 300 seconds. After cooling, it is molded again at 12 MPa and 175°C for 300 seconds, and water-cooled for 400 seconds to obtain a composite foam material.

[0061] Comparative Example 2

[0062] A method for preparing an EVA foam composite material specifically comprises the following steps:

[0063] 1) 90 parts by weight of EVA, 10 parts by weight of unmodified hydrotalcite, 0.4 parts by weight of stearic acid, 0.5 parts by weight of zinc stearate, 0.7 parts by weight of zinc oxide, 0.2 parts by weight of dicumyl peroxide and 2.5 parts by weight of AC were mixed and placed in a preheated extruder at a temperature of 110°C in each zone and a rotation speed of 20 rpm for 5 minutes;

[0064] 2) The mixture obtained in step 1) was quickly transferred to an open mill and mixed for 15 minutes, and then the material was pressed into 4 mm thin sheets;

[0065] 3) The sheet obtained in step 2) (the mass of the sheet is 1.2 times the volume of the mold in g / ml) is placed in the preheated flat vulcanizer cavity, and is molded and foamed at 12 MPa and 175°C for 300 seconds. After cooling, it is molded again at 12 MPa and 175°C for 300 seconds, and water-cooled for 400 seconds to obtain a composite foam material.

[0066] Comparative Example 3

[0067] A method for preparing an EVA foam composite material specifically comprises the following steps:

[0068] 1) 75 parts by weight of EVA, 10 parts by weight of unmodified polyvinyl alcohol, 5 parts by weight of unmodified graphene oxide, 10 parts by weight of unmodified hydrotalcite, 0.4 parts by weight of stearic acid, 0.5 parts by weight of zinc stearate, 0.7 parts by weight of zinc oxide, 0.2 parts by weight of dicumyl peroxide and 2.5 parts by weight of AC were mixed and placed in a preheated extruder, and the temperature of each zone was 110° C. and the speed was 20 rpm for extrusion and mixing for 5 minutes;

[0069] 2) The mixture obtained in step 1) was quickly transferred to an open mill and mixed for 15 minutes, and then the material was pressed into 4 mm thin sheets;

[0070] 3) The sheet obtained in step 2) (the mass of the sheet is 1.2 times the volume of the mold in g / ml) is placed in the preheated flat vulcanizer cavity, and is molded and foamed at 12 MPa and 175°C for 300 seconds. After cooling, it is molded again at 12 MPa and 175°C for 300 seconds, and water-cooled for 400 seconds to obtain a composite foam material.

[0071] Performance Testing

[0072] Figure 1 This is a molecular structure diagram of polyvinyl alcohol / oxidized expandable graphene / LDHs composite flame retardant. The LDHs composite flame retardant is firmly combined with the polyvinyl alcohol / oxidized expandable graphene composite flame retardant through electrostatic adsorption and hydrogen bonding, so the compatibility of the additive with the EVA matrix is ​​greatly improved. At the same time, guanidine urea phosphate cross-links with polyvinyl alcohol, and the phosphate and nitrate groups between the LDHs layers also significantly improve the flame retardant effect. And because of the excellent mechanical properties of graphene, the mechanical properties of the material are also significantly improved.

[0073] Figure 2 To prepare the XRD of LDHs composite flame retardant, the interlayer spacing of the composite flame retardant can be calculated by the Bragg formula to be 0.67nm, while the interlayer spacing of general LDHs materials is about 0.4nm.

[0074] Figure 3 For the preparation of LDHs composite flame retardant FT-IR, we can see 3500cm -1 1650cm -1 and 1200 cm -1 The corresponding amino, NH and CN characteristic peaks appear at 1380cm -1 and 1000 cm -1 The characteristic peaks of NO and PO corresponding to nitrate and phosphate ions appeared nearby, confirming the intercalation effect of phosphate and nitrate on LDHs.

[0075] Figure 4To prepare the SEM of PVA / oxidized expandable graphene / LDHs composite flame retardant, the results showed that the synthesized layered LDHs were adsorbed on the larger sheets of oxidized expandable graphene, resulting in LDHs@graphene@LDHs sandwich structure.

[0076] Table 1 Physical and mechanical properties of foam materials prepared in Examples and Comparative Examples

[0077]

[0078] Table 2 Flame retardant, wear resistance and anti-slip properties of foam materials prepared in Examples and Comparative Examples

[0079]

[0080] Tables 1 and 2 are the performance test results of each embodiment and comparative example. It can be clearly seen from the above physical and mechanical properties test results that in Examples 1 to 5, as the amount of composite flame retardant added increases, the tensile strength, tear strength and rebound are all improved compared to the comparative examples. Note that in Comparative Examples 1-3, unmodified polyvinyl alcohol, graphene oxide and hydrotalcite are listed respectively, and the ratio of 25 parts by weight of polyvinyl alcohol / oxidized expandable graphene / LDHs composite flame retardant added in Example 5 (polyvinyl alcohol / oxidized expandable graphene / LDHs: 41.7% / 20.8% / 37.5%) is compared after adding alone and adding together. The results show that due to the lack of cross-linking of guanidine urea phosphate, the grafting reaction of graphene oxide and polyvinyl alcohol, and the intercalation of phosphate and nitrate produced by betaine phosphate on LDHs, the mechanical properties such as tensile strength, elongation at break, tear strength, and flame retardant properties such as limiting oxygen index and vertical burning test of EVA foam materials are limited when unmodified additives are added alone or in combination. The addition of polyvinyl alcohol / oxidized expandable graphene / LDHs composite flame retardant significantly improves the mechanical properties, flame retardant properties, and wear and anti-skid properties of EVA foam materials. It is precisely because of the combined effects of guanidinium urea phosphate cross-linking modified polyvinyl alcohol, chemical grafting of graphene oxide and polyvinyl alcohol, and phosphate and nitrate produced by betaine phosphate on LDHs intercalation that a large number of amine and phosphate groups are added, which easily produce non-flammable acidic gases during combustion, promote polymer carbonization, and dilute oxygen in the air, thus greatly improving flame retardant properties. At the same time, guanidinium urea phosphate promotes the cross-linking of polyvinyl alcohol to improve toughness and rigidity, and provides a large number of hydrogen bond bridging sites, which greatly improves the compatibility of polyvinyl alcohol / oxidized expandable graphene / LDHs composite flame retardant in polymers, thereby better dispersing and avoiding the mechanical property attenuation caused by agglomeration when a large amount of additives are added. Due to the lack of physical barrier effect, when unmodified oxidized expandable graphene and unmodified hydrotalcite are added respectively, since both oxidized expandable graphene and hydrotalcite are flaky few-layer structures and lack support between layers, they are prone to stacking and agglomeration during mechanical processing, thus affecting the performance effect.

[0081] It can be seen that the composite additive of the present invention is an EVA foam composite material which not only maintains the basic mechanical properties of the original material, but also greatly improves the tensile strength and tear strength, and has excellent anti-slip properties. It can still greatly improve the dynamic friction coefficient (DCOF) in the case of a small amount of addition, which not only saves production costs, but also reduces dust during processing and is beneficial to the environment. It also has excellent flame retardant properties.

[0082] The above description is only a preferred embodiment of the present invention. All equivalent changes and modifications made according to the scope of the patent application of the present invention should fall within the scope of the present invention.

Claims

1. A degradable flame-retardant and wear-resistant composite foam material, characterized in that: The raw material composition of the degradable flame-retardant and wear-resistant composite foam material includes, by weight: 75-95 parts of ethylene-vinyl acetate copolymer, 5-25 parts of polyvinyl alcohol / oxidized expandable graphene / LDHs composite flame retardant, 2.5-3 parts of foaming agent AC, 0.2-1 part of cross-linking agent DCP, and 1-2 parts of stearic acid+zinc stearate+zinc oxide; The preparation method of the polyvinyl alcohol / oxidized expandable graphene / LDHs composite flame retardant comprises the following steps: 1) Preparation of oxidized expandable graphene: 3 g of expandable graphite was added to 150 ml of concentrated sulfuric acid, stirred at room temperature for 1 h under high-speed magnetic stirring, and then 5 g of potassium permanganate was slowly added, reacted for 2 h, heated to 90°C, and 150 ml of deionized water and 50 ml of 30 wt.% hydrogen peroxide solution were added respectively, and finally centrifuged several times in a centrifuge at 8000 rpm, washed, and dried to obtain oxidized expandable graphene; 2) Preparation of LDHs composite flame retardant: Magnesium nitrate hexahydrate and aluminum nitrate nonahydrate were added into a three-necked flask at a molar ratio of 3:1, and then deionized water was added to dissolve. The three-necked flask was placed in a water bath and heated to 80°C, and stirred continuously. Betaine phosphate was then added, and stirring continued for 3 hours. The mixture was filtered, dried, and ground for later use. 3) Preparation of polyvinyl alcohol / oxidized expandable graphene composite flame retardant: 1 g of polyvinyl alcohol, 200 mg of guanidine urea phosphate, 2 ml of 10 wt.% HCl solution and 500 mg of oxidized expandable graphene were dissolved in 200 ml of deionized water, heated to 80°C, mixed for 3 h, centrifuged several times, dried and crushed for later use; 4) Preparation of polyvinyl alcohol / oxidized expandable graphene / LDHs composite flame retardant: 5 g of polyvinyl alcohol / oxidized expandable graphene composite flame retardant was ultrasonically dispersed in deionized water, and then 3 g of LDHs composite flame retardant was added. The mixture was stirred continuously, and when a flocculent precipitate was produced, it was quickly filtered and dried for later use.

2. The degradable flame-retardant and wear-resistant composite foam material according to claim 1, characterized in that: The molar ratio of betaine phosphate to the sum of magnesium nitrate hexahydrate and aluminum nitrate nonahydrate is 1:

1.

3. The degradable flame-retardant and wear-resistant composite foam material according to claim 1, characterized in that: The content of vinyl acetate in the ethylene-vinyl acetate copolymer is 13wt%-20wt%.

4. A method for preparing the degradable flame retardant and wear resistant composite foam material according to any one of claims 1 to 3, characterized in that: The following steps are involved: 1) Ethylene-vinyl acetate copolymer, polyvinyl alcohol / oxidized expandable graphene / LDHs composite flame retardant, stearic acid, crosslinking agent DCP and foaming agent AC were mixed evenly and placed in a preheated internal mixer at a heating temperature of 110-120°C and a speed of 20 rpm for 5 minutes; 2) The mixture obtained in step 1) is quickly transferred to an open mill and kneaded for 10-20 minutes, and then the material is pressed into 3-5 mm thin sheets; 3) placing the sheet obtained in step 2) in a preheated flat vulcanizing machine cavity, performing compression molding and foaming at 12 MPa and 175° C. for 300 seconds, and then performing secondary oil pressure molding at 12 MPa and 175° C. for 300 seconds, and water cooling for 400 seconds to obtain a biodegradable flame retardant and wear-resistant composite foam material.