One-element waterproof self-spraying paint and its preparation method and application

Through the combination of waterproof coating with specific components and high-efficiency propellant, the storage stability and construction uniformity problems of waterproof self-spraying paint are solved, efficient waterproof coating effect is achieved, paint waste is reduced and waterproof performance is improved.

CN116355480BActive Publication Date: 2024-10-11WANCAN TECH (SHANGHAI) CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310439242.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-04-23
Publication Date
2024-10-11
Estimated Expiration
2043-04-23

AI Technical Summary

Technical Problem

Existing waterproof self-spray paint has problems with poor stability and poor uniform coating during storage and construction, resulting in paint waste and unsatisfactory waterproofing effects.

Method used

A combination of waterproof coatings with specific components and high-efficiency environmentally friendly propellants, including film-forming emulsions, powdery thickeners, liquid thickeners, dispersants, defoaming agents and surfactants, compounded by anionic and nonionic emulsifiers. Formulated to form a stable emulsion system, paired with a spray pressure tank to ensure storage stability and construction results.

Benefits of technology

It achieves excellent storage stability and good construction effect of waterproof coating, reduces paint waste, ensures uniform coating, and improves waterproof performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004193272280000021
    Figure BDA0004193272280000021
  • Figure BDA0004193272280000031
    Figure BDA0004193272280000031
  • Figure BDA0004193272280000081
    Figure BDA0004193272280000081
Patent Text Reader

Abstract

The invention provides a one-unit waterproof self-spraying paint and a preparation method and application thereof. The one-unit waterproof self-spraying paint comprises a combination of a waterproof coating, a propellant and a spray pressure tank. The waterproof coating comprises a combination of a specific number of film-forming emulsions, film-forming aids, powdered thickeners, liquid thickeners, dispersants, defoamers, surfactants and water. By limiting the film-forming emulsion to include an acrylate copolymer emulsion and / or a styrene-acrylic emulsion and matching the specific aids, the obtained waterproof coating has excellent mechanical properties. The one-unit waterproof self-spraying paint is matched with a propellant and loaded into a spray pressure tank, so that the obtained one-unit waterproof self-spraying paint has excellent storage stability and good construction effect, is convenient for construction under various conditions, can achieve a uniform coating effect, and has less waste of coating.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of waterproof coatings, and specifically relates to a one-element waterproof self-spraying paint and a preparation method and application thereof. Background Art

[0002] At present, local water seepage in buildings often occurs. The use of waterproof coatings is the most convenient and effective in conventional waterproofing measures. The amount of coating used for local repairs is relatively small. Most of the coatings sold on the market are barreled. The use of remaining coatings will result in waste. In addition, it is difficult to achieve uniform coating of the internal corners and leaks at the pipe joints by roller coating and brush coating, which affects the waterproof effect. The existing spraying method requires the use of a large number of construction tools. Waterproof coating refers to a coating that forms a coating film that can prevent rainwater or groundwater from leaking. Waterproof coatings can be divided into emulsion type, solvent type, reactive type and modified asphalt according to the state and form of the coating. The waterproof film formed by the waterproof coating after curing has certain elongation, elastic-plasticity, crack resistance, impermeability and weather resistance, and can play a role in waterproofing, anti-seepage and protection.

[0003] Spray paint is a kind of paint that is processed by special methods and then filled into the spray paint bottle under high pressure, which is convenient for users to spray. Spray paint bottles usually include a bottle body and an aerosol valve. The bottle body is filled with paint and propellant. When using it, press the aerosol valve to spray. It is simple and convenient to use. CN105907201A discloses an environmentally friendly water-based self-spraying paint comprising an environmentally friendly water-based self-spraying paint liquid, a propellant, and an aerosol packaging material, and a preparation method thereof. The liquid comprises the following components in parts by weight: 30 to 45 parts of water-based resin, 5 to 15 parts of pigment, 15 to 30 parts of cosolvent, 20 to 35 parts of water, and 0.5 to 2 parts of additives. The environmentally friendly water-based self-spraying paint liquid provided by the invention adopts a water-based resin system, and the entire paint film has good water- and oil-repellent effects, which helps to improve the quality of the self-spraying paint product; part of the water is used to replace part of the solvent to reduce VOC, which is environmentally friendly and in line with the concept of environmental protection; the produced environmentally friendly water-based self-spraying paint has good spray atomization, high spraying rate, rapid film drying, high film fullness, excellent comprehensive properties such as hardness, adhesion, gloss, flexibility, and impact resistance, rich and bright colors, excellent decorative effect, good aging resistance, and excellent anti-rust and protective functions. However, the propellant used in the above invention is an organic gas with a pungent odor, which is not environmentally friendly; the prepared coating has poor storage performance in the tank, has a hard bottoming phenomenon, and cannot be used; the spraying construction effect is poor, it is impossible to achieve uniform construction, and there is a serious situation of local material accumulation; the spraying has serious bubbles on the wall, which seriously affects the density of the dry film and cannot achieve the effect of waterproofing and leak plugging.

[0004] Therefore, developing a one-component waterproof self-spray paint with excellent storage stability and uniform coating is a technical problem that needs to be solved urgently in this field. Summary of the invention

[0005] In view of the deficiencies in the prior art, the object of the present invention is to provide a one-unit waterproof self-spraying paint and a preparation method and application thereof. The one-unit waterproof self-spraying paint comprises a waterproof coating, a propellant and a spray pressure tank. By selecting a waterproof coating of a specific component and a high-efficiency and environmentally friendly propellant for combination, the obtained one-unit waterproof self-spraying paint has excellent storage stability and good construction effect, is convenient for construction under various conditions, has less paint waste, and can achieve uniform coating.

[0006] To achieve this object, the present invention adopts the following technical solutions:

[0007] In a first aspect, the present invention provides a one-piece waterproof self-spraying paint, the one-piece waterproof self-spraying paint comprising a waterproof coating, a propellant and a spray pressure tank;

[0008] The waterproof coating comprises the following components in parts by weight:

[0009]

[0010]

[0011] The film-forming emulsion includes acrylate copolymer emulsion and / or styrene acrylic emulsion.

[0012] Wherein, the film-forming emulsion may be 310 parts by weight, 320 parts by weight, 330 parts by weight, 340 parts by weight or 350 parts by weight, etc.

[0013] The film-forming aid may be 6 parts by weight, 7 parts by weight, 8 parts by weight, 9 parts by weight, or 10 parts by weight.

[0014] The powdered thickener may be 1.5 parts by weight, 2 parts by weight, 2.5 parts by weight, 3 parts by weight, 3.5 parts by weight, etc.

[0015] The liquid thickener may be 1.2 parts by weight, 1.4 parts by weight, 1.6 parts by weight, 1.8 parts by weight, 2 parts by weight, 2.2 parts by weight, 2.4 parts by weight, 2.6 parts by weight, 2.8 parts by weight, etc.

[0016] The dispersant may be 12 parts by weight, 14 parts by weight, 16 parts by weight, 18 parts by weight, etc.

[0017] The defoaming agent can be 1.5 parts by weight, 2 parts by weight, 2.5 parts by weight, 3 parts by weight or 3.5 parts by weight, etc.

[0018] The surfactant may be 2.5 parts by weight, 3 parts by weight, 3.5 parts by weight, 4 parts by weight, 4.5 parts by weight, 5.5 parts by weight, etc.

[0019] The water may be 170 parts by weight, 180 parts by weight, 190 parts by weight, 200 parts by weight, etc.

[0020] The one-component waterproof self-spraying paint provided by the present invention comprises a combination of a waterproof coating, a propellant and a spray pressure tank, wherein the waterproof coating comprises a combination of a specific number of film-forming emulsions, film-forming aids, powdered thickeners, liquid thickeners, dispersants, defoamers, surfactants and water, and the film-forming emulsion is limited to include an acrylate copolymer emulsion and / or a styrene-acrylic emulsion, and is matched with the above-mentioned specific aids, so that the obtained waterproof coating has excellent mechanical properties, and at the same time, because the film-forming emulsion is emulsified by an emulsification system compounded with an anionic emulsifier and a nonionic emulsifier, The film-forming emulsion has higher storage stability under high pressure and polar gas conditions; at the same time, through the synergistic effect of the powdered thickener and the surfactant, a gel protective layer is formed on the outer layer of the latex particles of the film-forming emulsion, so that the latex particles can stably exist under the conditions of the spray paint can for a long time. Finally, the one-unit waterproof spray paint obtained by combining the above-mentioned waterproof coating with a specific number of propellants and loading it into a spray pressure can has excellent storage stability and good construction effect, is convenient for construction under various construction conditions, has less paint waste, and can achieve the advantage of uniform coating.

[0021] Preferably, the mass ratio of the propellant to the waterproof coating is 1:(2-5), for example, 1:2.5, 1:3, 1:3.5, 1:4, 1:4.5 or 1:5, etc.

[0022] Preferably, the glass transition temperature of the film-forming emulsion is less than 0°C, for example, -5°C, -10°C, -15°C, -20°C, -25°C, -28°C, -26°C, -24°C or -22°C.

[0023] Preferably, the particle size distribution of the latex particles in the film-forming emulsion is 200-300 nm, for example, 210 nm, 220 nm, 230 nm, 240 nm, 250 nm, 260 nm, 270 nm, 280 nm or 290 nm.

[0024] Preferably, the pH value of the film-forming emulsion is 5-6, such as 5.2, 5.4, 5.6 or 5.8.

[0025] Preferably, the film-forming emulsion is obtained by emulsifying an anionic emulsifier and a nonionic emulsifier together.

[0026] As a preferred technical solution of the present invention, a film-forming emulsion having a glass transition temperature of less than 0°C and emulsified with an anionic emulsifier and a nonionic emulsifier is selected. The advantage is that the obtained film-forming emulsion can be stably present in a spray pressure tank containing a propellant without demulsification. If the glass transition temperature of the selected film-forming emulsion is not within the above range, the obtained waterproof coating will not be able to achieve excellent mechanical properties under specific use environments, such as insufficient elongation under low temperature conditions leading to cracking, etc.; if only a film-forming emulsion obtained by emulsification with an anionic emulsifier is selected, the obtained film-forming emulsion will be unstable in the propellant atmosphere and easily demulsified, making the final self-spraying paint product unusable; if only a film-forming emulsion obtained by emulsification with a nonionic emulsifier is selected, the obtained film-forming emulsion will be unstable in the propellant atmosphere and easily demulsified, making the final self-spraying paint product unusable.

[0027] Preferably, the film-forming aid comprises dodecyl alcohol ester and / or diethylene glycol monobutyl ether.

[0028] Preferably, the powdered thickener includes any one of hydroxyethyl cellulose ether, attapulgite or bentonite, or a combination of at least two of them.

[0029] Preferably, the liquid thickener includes a swelling thickener and / or a polyurethane thickener.

[0030] Preferably, the dispersant comprises a sodium salt anionic dispersant.

[0031] Preferably, the defoaming agent comprises a mineral oil type defoaming agent and / or a silicone type defoaming agent.

[0032] Preferably, the surfactant comprises a nonionic surfactant.

[0033] Preferably, the nonionic surfactant includes any one of alkylphenol polyoxyethylene ether, high-carbon fatty alcohol polyoxyethylene ether, fatty acid methyl ester ethoxylate or alkyl alcohol amide, or a combination of at least two thereof.

[0034] Preferably, the water is deionized water, which is obtained by removing ionic impurities in water through an ion exchange device.

[0035] Preferably, the waterproof coating further comprises any one of a pH regulator, an antifreeze agent or a pigment or filler, or a combination of at least two of them.

[0036] Preferably, the content of the pH regulator in the waterproof coating is 1 to 3 parts by weight, for example, 1.2 parts by weight, 1.4 parts by weight, 1.6 parts by weight, 1.8 parts by weight, 2 parts by weight, 2.2 parts by weight, 2.4 parts by weight, 2.6 parts by weight or 2.8 parts by weight.

[0037] Preferably, the pH adjuster includes aqueous ammonia, and commercially available AMP-95 can be selected.

[0038] Preferably, the content of antifreeze agent in the waterproof coating is 15 to 25 parts by weight, for example, 16 parts by weight, 17 parts by weight, 18 parts by weight, 19 parts by weight, 20 parts by weight, 21 parts by weight, 22 parts by weight, 23 parts by weight or 24 parts by weight.

[0039] Preferably, the antifreeze agent comprises propylene glycol.

[0040] Preferably, the content of pigments and fillers in the waterproof coating is 400 to 500 parts by weight, for example, 420 parts by weight, 440 parts by weight, 460 parts by weight or 480 parts by weight.

[0041] Preferably, the pigment and filler include any one of titanium dioxide, quartz powder, heavy calcium carbonate or talcum powder, or a combination of at least two of them.

[0042] Preferably, the propellant includes any one of dimethyl ether, propane, butane or difluoroethane, or a combination of at least two thereof.

[0043] Preferably, the spray pressure tank comprises a tank body, an aerosol valve and a press spray head.

[0044] Preferably, the can body is made of aluminum.

[0045] Preferably, the minimum deformation pressure of the spray pressure tank is 1.2-2.0 MPa, for example, 1.3 MPa, 1.4 MPa, 1.5 MPa, 1.6 MPa, 1.7 MPa, 1.8 MPa or 1.9 MPa.

[0046] In a second aspect, the present invention provides a method for preparing the one-component waterproof self-spraying paint as described in the first aspect, the preparation method comprising the following steps:

[0047] (1) mixing water, a powdered thickener, a dispersant, a portion of a defoaming agent, a surfactant, an optional pH thickener, an optional antifreeze agent, and an optional pigment to obtain a first mixture;

[0048] (2) mixing the first mixture obtained in step (1), the film-forming emulsion, the film-forming aid, the remaining part of the defoamer and the liquid thickener to obtain a waterproof coating;

[0049] (3) Add the waterproof coating obtained in step (2) into a spray pressure tank, then fill the propellant into the self-spray paint bottle by the under-cap filling method, and seal the bottle, connect the press nozzle, and obtain the one-unit waterproof self-spray paint.

[0050] Preferably, the mixing in step (1) specifically comprises: first mixing for 5 to 10 min (for example, 5.5 min, 6 min, 6.5 min, 7 min, 7.5 min, 8 min, 8.5 min, 9 min or 9.5 min, etc.) at a stirring condition of 300 to 500 rpm (for example, 320 rpm, 340 rpm, 360 rpm or 380 rpm, etc.), and then mixing for 20 to 25 min (for example, 21 min, 22 min, 23 min or 24 min, etc.) at a stirring condition of 1000 to 1400 rpm (for example, 1050 rpm, 1100 rpm, 1150 rpm, 1200 rpm, 1250 rpm, 1300 rpm or 1350 rpm, etc.) to complete the mixing.

[0051] Preferably, the mixing in step (2) is carried out under stirring conditions at a rotation speed of 600 to 800 rpm (e.g., 620 rpm, 640 rpm, 660 rpm, 680 rpm, 700 rpm, 720 rpm, 740 rpm, 760 rpm or 780 rpm, etc.).

[0052] Preferably, the mixing time in step (2) is 5 to 10 minutes, for example, 6 minutes, 7 minutes, 8 minutes, 9 minutes or 10 minutes.

[0053] In a third aspect, the present invention provides a use of the one-component waterproof self-spraying paint as described in the first aspect in local repair.

[0054] Compared with the prior art, the present invention has the following beneficial effects:

[0055] The one-unit waterproof self-spraying paint provided by the present invention comprises a combination of a waterproof coating, a propellant and a spray pressure tank, wherein the waterproof coating comprises a combination of a specific number of film-forming emulsions, film-forming aids, powdered thickeners, liquid thickeners, dispersants, defoamers, surfactants and water. By limiting the film-forming emulsion to include an acrylate copolymer emulsion and / or a styrene-acrylic emulsion, and matching the above-mentioned specific aids, the obtained waterproof coating has excellent mechanical properties, and then when matched with a propellant and loaded into a spray pressure tank, it has excellent storage stability and good construction effect, is convenient for construction under various construction conditions, and at the same time has the advantages of less paint waste and uniform coating. DETAILED DESCRIPTION

[0056] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.

[0057] The information of some raw materials involved in the specific implementation of the present invention is as follows:

[0058] Film-forming emulsion: Dow Chemical, Tianba 2012; Badfu, FS-320A; Badfu, FS-670;

[0059] The film-forming aid is Texanol, sourced from Eastman;

[0060] The powdered thickener is hydroxyethyl cellulose ether;

[0061] The liquid thickener used is TT-615, which comes from Dow Chemical;

[0062] The dispersant used was SN5040, from Nopco;

[0063] The defoamer used is NXZ, which comes from BASF;

[0064] The surfactant used was DOWFAX X-405, sourced from Rohm and Haas;

[0065] The pH regulator is ammonia water;

[0066] The antifreeze is propylene glycol;

[0067] The pigment and filler is titanium dioxide.

[0068] Example 1

[0069] A one-piece waterproof self-spraying paint, comprising a waterproof coating, a propellant and a spray pressure tank;

[0070] The waterproof coating comprises the following components in parts by weight:

[0071]

[0072] The propellant is dimethyl ether, and the mass ratio of dimethyl ether to waterproof coating is 1:3;

[0073] The spray pressure tank includes an aluminum tank body, an aerosol valve and a press-type nozzle, and the minimum deformation pressure is 1.8 MPa;

[0074] The preparation method of the one-element waterproof self-spraying paint provided in this embodiment comprises the following steps:

[0075] (1) mixing deionized water, a powdered thickener, a pH regulator, a dispersant, 1 / 2 of a defoamer, a surfactant, an antifreeze agent, and a pigment and filler at a rotation speed of 400 rpm for 10 minutes, and then dispersing the mixture at a stirring speed of 1200 rpm for 20 minutes to obtain a first mixture;

[0076] (2) mixing the first mixture obtained in step (1), the film-forming emulsion, the film-forming aid, the remaining 1 / 2 of the defoamer and the liquid thickener at 700 rpm for 10 minutes to obtain a waterproof coating;

[0077] (3) Add the waterproof coating obtained in step (3) into a spray pressure tank, then fill the propellant into the spray pressure tank by mechanical filling through a method of filling under the cover, and seal the tank, and finally connect a press nozzle to obtain the one-unit waterproof self-spraying paint.

[0078] Example 2

[0079] A one-piece waterproof self-spraying paint, comprising a waterproof coating, a propellant and a spray pressure tank;

[0080] The waterproof coating comprises the following components in parts by weight:

[0081]

[0082] The propellant is propane, and the mass ratio of propane to waterproof coating is 1:5;

[0083] The spray pressure tank includes an aluminum tank body, an aerosol valve and a press-type nozzle, and the minimum deformation pressure is 1.8 MPa;

[0084] The other raw materials and preparation method of the one-component waterproof self-spraying paint provided in this embodiment are the same as those in Example 1.

[0085] Example 3

[0086] A one-piece waterproof self-spraying paint, comprising a waterproof coating, a propellant and a spray pressure tank;

[0087] The waterproof coating comprises the following components in parts by weight:

[0088]

[0089] The propellant is butane, and the mass ratio of butane to waterproof coating is 1:2;

[0090] The spray pressure tank includes an aluminum tank body, an aerosol valve and a press-type nozzle, and the minimum deformation pressure is 1.8 MPa;

[0091] The other raw materials and preparation method of the one-component waterproof self-spraying paint provided in this embodiment are the same as those in Example 1.

[0092] Example 4

[0093] A one-piece waterproof self-spraying paint, comprising a waterproof coating, a propellant and a spray pressure tank;

[0094] The waterproof coating comprises the following components in parts by weight:

[0095]

[0096] The propellant is difluoroethane, and the mass ratio of difluoroethane to the waterproof coating is 1:4;

[0097] The spray pressure tank includes an aluminum tank body, an aerosol valve and a press-type nozzle, and the minimum deformation pressure is 1.8 MPa;

[0098] The other raw materials and preparation method of the one-component waterproof self-spraying paint provided in this embodiment are the same as those in Example 1.

[0099] Example 5

[0100] A one-component waterproof self-spraying paint, which differs from Example 1 only in that a film-forming emulsion (Badford, FS-320A) is used to replace a film-forming emulsion (Dow Chemical, Tianba 2012), and other components, amounts and preparation methods are the same as those in Example 1.

[0101] Example 6

[0102] A one-component waterproof self-spraying paint, which differs from Example 1 only in that a film-forming emulsion (Badford, FS-670) is used to replace a film-forming emulsion (Dow Chemical, Tianba 2012), and other components, amounts and preparation methods are the same as those in Example 1.

[0103] Comparative Example 1

[0104] A one-component waterproof self-spraying paint, which differs from Example 1 only in that no surfactant is added, and other components, dosages and preparation methods are the same as those in Example 1.

[0105] Comparative Example 2

[0106] A one-component waterproof self-spraying paint, which differs from Example 1 only in that the added amount of the surfactant is 8 parts by weight, and the other components, amounts and preparation methods are the same as those in Example 1.

[0107] Comparative Example 3

[0108] A one-component waterproof self-spraying paint, which differs from Example 1 only in that the mass ratio of the propellant to the waterproof coating is 1:6, and other components, dosages and preparation methods are the same as those in Example 1.

[0109] Comparative Example 4

[0110] A one-component waterproof self-spraying paint, which differs from Example 1 only in that the mass ratio of the propellant to the waterproof coating is 1:1, and other components, dosages and preparation methods are the same as those in Example 1.

[0111] Performance Testing:

[0112] (1) Tensile strength, elongation at break, low temperature flexibility and water impermeability: Tested according to the test methods provided in JC / T 864-2008.

[0113] The waterproof coatings provided in Examples 1 to 6 and Comparative Examples 1 to 4 were tested according to the above test method. The test results are shown in Table 1:

[0114] Table 1

[0115]

[0116] According to the data in Table 1, we can see that:

[0117] The waterproof coating provided in Examples 1 to 4 has a tensile strength of 1.96 to 2.11 MPa before heating and an elongation at break of 469 to 882%. The tensile strength after heat treatment is 5.94 to 6.75 MPa and the elongation at break is 206 to 225%. The low-temperature flexibility test shows that there are no cracks at -10°C, and the water-impermeability test shows that they are all water-impermeable.

[0118] However, in Example 1, no surfactant was added, in Example 2, too much surfactant was added, in Example 3, too little propellant was added, and in Example 4, too much propellant was added, all of which would have an adverse effect on the tensile strength and elongation at break of the waterproof coating.

[0119] Compared with Example 1, Examples 5 to 6 change the type of film-forming emulsion, which also affects the performance of the final waterproof coating.

[0120] (2) Construction performance: The one-unit waterproof self-spraying paint provided in Examples 1 to 6 and Comparative Examples 1 to 4 was subjected to construction tests, and heat storage was performed at 50° C., spraying tests were performed after 1 week and 1 month, and low temperature (5° C.) storage for 24 hours was performed. The obtained data are shown in Table 2 below:

[0121] Table 2

[0122]

[0123]

[0124] According to the data in Table 2, we can see that:

[0125] The one-element waterproof self-spraying paint provided in Examples 1 to 4 has excellent construction characteristics and storage stability, and is normal when sprayed directly, stored in hot water for 1 week or 1 month, or stored at low temperature for 24 hours.

[0126] However, in comparative example 1, the one-component waterproof self-spray paint without adding surfactant showed a small amount of colloid particles when sprayed after one week of hot storage, accompanied by the coarsening of pigments and fillers. Moreover, a large amount of colloid particles were also sprayed out when sprayed after 24 hours of low-temperature storage, accompanied by the coarsening of pigments and fillers, indicating that the low-temperature storage and hot storage performances are poor.

[0127] In comparative example 2, the one-component waterproof self-spray paint with excessive surfactant addition will spray out a small amount of large colloidal particles when sprayed after being hot stored for one month, which also indicates that the heat storage performance is poor.

[0128] In comparative example 3, too little propellant added seriously affects the spraying effect of the one-yuan waterproof spray paint. Large particle fog points will appear during direct spraying, and the atomization effect is poor.

[0129] In comparative example 4, the one-component waterproof self-spray paint with excessive propellant addition had a small amount of colloidal particles when sprayed after one week of heat storage, accompanied by the coarsening of the pigment and filler, indicating that the heat storage performance was poor.

[0130] The applicant declares that the present invention illustrates a one-component waterproof self-spraying paint and its preparation method and application through the above-mentioned embodiments, but the present invention is not limited to the above-mentioned embodiments, that is, it does not mean that the present invention must rely on the above-mentioned embodiments to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of the raw materials of the product of the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.

Claims

1. A one-element waterproof self-spraying paint, characterized in that: The one-piece waterproof self-spraying paint comprises a waterproof coating, a propellant and a spray pressure tank; The waterproof coating comprises the following components in parts by weight: The film-forming emulsion is Dow Chemical Tianba 2012; The mass ratio of the propellant to the waterproof coating is 1:(2-5); The surfactant includes any one of alkylphenol polyoxyethylene ether, high-carbon fatty alcohol polyoxyethylene ether, fatty acid methyl ester ethoxylate or alkyl alcohol amide, or a combination of at least two thereof.

2. The one-piece waterproof self-spraying paint according to claim 1, characterized in that: The film-forming aid includes dodecyl alcohol ester and / or diethylene glycol monobutyl ether.

3. The one-piece waterproof self-spraying paint according to claim 1, characterized in that: The powdered thickener includes any one of hydroxyethyl cellulose ether, attapulgite or bentonite, or a combination of at least two of them.

4. The one-piece waterproof self-spraying paint according to claim 1, characterized in that: The liquid thickener includes a swelling thickener and / or a polyurethane thickener.

5. The one-piece waterproof self-spraying paint according to claim 1, characterized in that: The dispersant includes a sodium salt anionic dispersant.

6. The one-piece waterproof self-spraying paint according to claim 1, characterized in that: The defoaming agent includes a mineral oil type defoaming agent and / or a silicone type defoaming agent.

7. The one-piece waterproof self-spraying paint according to claim 1, characterized in that: The water is deionized water.

8. The one-piece waterproof self-spraying paint according to claim 1, characterized in that: The waterproof coating also includes any one of a pH regulator, an antifreeze agent or a pigment or filler, or a combination of at least two of them.

9. The one-piece waterproof self-spraying paint according to claim 8, characterized in that: The content of the pH regulator in the waterproof coating is 1 to 3 parts by weight.

10. The one-piece waterproof self-spraying paint according to claim 8, characterized in that: The pH adjuster includes aqueous ammonia.

11. The one-piece waterproof self-spraying paint according to claim 8, characterized in that: The content of the antifreeze agent in the waterproof coating is 15 to 25 parts by weight.

12. The one-piece waterproof self-spraying paint according to claim 8, characterized in that: The antifreeze agent includes propylene glycol.

13. The one-piece waterproof self-spraying paint according to claim 8, characterized in that: The content of pigment and filler in the waterproof coating is 400 to 500 parts by weight.

14. The one-piece waterproof self-spraying paint according to claim 8, characterized in that: The pigment and filler include any one of titanium dioxide, quartz powder, heavy calcium carbonate or talcum powder, or a combination of at least two of them.

15. The one-piece waterproof self-spraying paint according to claim 1, characterized in that: The propellant includes any one of dimethyl ether, propane, butane or difluoroethane, or a combination of at least two thereof.

16. The one-yuan waterproof self-spraying paint according to claim 1, characterized in that: The spray pressure tank comprises a tank body, an aerosol valve and a press spray head.

17. The one-piece waterproof self-spraying paint according to claim 16, characterized in that: The material of the tank body is aluminum.

18. The one-yuan waterproof self-spraying paint according to claim 1, characterized in that: The minimum deformation pressure of the spray pressure tank is 1.2-2.0 MPa.

19. A method for preparing the one-component waterproof self-spraying paint according to any one of claims 1 to 18, characterized in that: The preparation method comprises the following steps: (1) mixing water, a powdered thickener, a dispersant, a portion of a defoaming agent, a surfactant, an optional pH thickener, an optional antifreeze agent, and an optional pigment to obtain a first mixture; (2) mixing the first mixture obtained in step (1), the film-forming emulsion, the film-forming aid, the remaining part of the defoamer and the liquid thickener to obtain a waterproof coating; (3) Add the waterproof coating obtained in step (2) into a spray pressure tank, then fill the propellant into the spray pressure tank by filling under the cover, and seal the tank, connect the press nozzle, and obtain the one-unit waterproof self-spraying paint.

20. The preparation method according to claim 19, characterized in that: The mixing in step (1) specifically includes: first mixing at a stirring speed of 300 to 500 rpm for 5 to 10 minutes, and then mixing at a stirring speed of 1000 to 1400 rpm for 20 to 25 minutes to complete the mixing.

21. The preparation method according to claim 19, characterized in that: The mixing in step (2) is carried out under stirring conditions at a rotation speed of 600 to 800 rpm.

22. The preparation method according to claim 19, characterized in that: The mixing time in step (2) is 5 to 10 minutes.

23. Use of the one-component waterproof self-spraying paint as claimed in any one of claims 1 to 18 in local repair.