A method for preparing a cation-doped modified lithium ion sieve
Through the cationically doped modified lithium manganese oxide preparation method, the problem of insufficient performance of lithium manganese oxide adsorbent is solved, and efficient lithium ion adsorption and stability are achieved, which is suitable for industrial production.
Patent Information
- Application Number
- CN202310175726.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-02-28
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2043-02-28
AI Technical Summary
The existing lithium manganese oxide adsorbents have shortcomings in lithium ion adsorption and regeneration properties, and the synthesis process is complicated, making it difficult to achieve industrial production.
The preparation method of lithium manganese oxides modified by cationic doping is adopted. The target doped element salt is mixed with the manganese salt by hydrothermal method, and then reacted with the lithium salt after calcination to form the lithium ion sieve precursor, and then carried out pickling treatment to obtain Lithium ion sieve with high adsorption properties and stability.
High selectivity and high purity adsorption of lithium ions are achieved, the manganese dissolution rate is reduced, the circulation stability of the material and the feasibility of industrial production are improved.
Smart Images

Figure CN116371387B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of ion sieve preparation, and in particular relates to a method for preparing a cation-doped modified lithium ion sieve. Background Art
[0002] Lithium and its derivatives, in the form of ceramics or glass, play a key role in a variety of commercial applications such as batteries, pharmaceuticals, and lubricants, and have become strategic technological elements. The global demand for lithium resources has increased dramatically due to the increased demand for electronic devices and electric vehicles. At present, the main resources of lithium are brine deposits in South America (Chile, Bolivia and Argentina), followed by hard rock resources. Among these lithium resources, continental brine resources account for the largest proportion except for seawater. Therefore, it is very important to separate and extract lithium ions from these resources. Lithium ion sieve technology can achieve high adsorption capacity, high lithium selectivity, environmental friendliness and obtain high-purity lithium products. From the perspective of the metal transition skeleton, lithium ion sieve can be mainly obtained from two precursor materials, namely lithium manganese oxide and lithium titanium oxide. Compared with lithium titanium oxide, spinel lithium manganese oxide has the advantages of large lithium adsorption capacity, good regeneration performance and simple synthesis, and is the most widely used precursor material. Among them, Li 1.6 Mn 1.6 O4 has a high theoretical adsorption capacity and a low Mn loss rate, so it is the main adsorbent for lithium recovery in solution. Trace doping can further improve its performance and cycle stability. Chitrakar et al. synthesized Li4Fe x Mn 5-x O 12 The results show that as the Fe / Mn ratio increases, the dissolution of Mn decreases and the Li + However, element doping has an effect on the adsorption of Li 1.6 Mn 1.6 O4 adsorption of Li + There are few studies on this. The patent application with publication number CN103991908A discloses a method for regulating the stability of lithium ion sieves by cation doping. The solid phase method is used to 12 Composite oxides are doped with metal ions. 1.6 Mn 1.6 O4 cannot be directly synthesized, so LiMnO2 is first synthesized through a hydrothermal reaction, and then LiMnO2 is calcined at low temperature in an air atmosphere. There is no literature report on the one-step preparation of uniformly doped lithium manganese oxide. Summary of the invention
[0003] The purpose of the present invention is to provide a method for preparing a cation-doped modified lithium ion sieve.
[0004] In order to achieve the above object, the technical solution adopted by the present invention is as follows:
[0005] The first aspect of the present invention provides a method for preparing a cation-doped modified lithium ion sieve, comprising the following steps:
[0006] Step 1: ultrasonically dissolve the target doping element salt in the solvent, slowly pour in the manganese salt after it is fully dissolved and continue ultrasonication for 1 to 5 hours, dry at 50 to 80 ° C for 1 to 12 hours, and then calcine at 500 to 800 ° C for 3 to 12 hours in an air atmosphere to obtain metal-doped modified Mn 2-x R x O3;
[0007] Alternatively, the target doping element salt and the manganese salt are mixed evenly, and calcined at 500-800°C for 3-12 hours in an air atmosphere to obtain a metal-doped modified Mn 2-x R x O3;
[0008] In the target doping element salt and manganese salt, the molar ratio of R to Mn is (0.01-0.18):1;
[0009] Metal doped modified Mn 2-x R x O3, lithium salt grinding and mixing, Mn 2-x R x The molar ratio of Li to Mn in O3 and lithium salt is (1-1.2):1; fully react at a temperature of 100-180°C for 1-72 hours, and dry to obtain LiMn 1-x R x O2 powder;
[0010] The target doping element salt is selected from the acetate, sulfate, nitrate or carbonate of at least one of the following elements: Ti, Fe, Co, Cu, Ni, Zn, Zr, Ce;
[0011] The manganese salt is selected from at least one of manganese acetate, manganese carbonate, manganese sulfate, manganese dioxide, and manganese iodide;
[0012] The lithium salt is selected from at least one of LiOH·H2O, LiNO3 or Li2CO3;
[0013] Step 2: LiMn obtained in the first step 1-x R x The O2 powder is calcined at 300-500°C in an air atmosphere for 4-72 hours to obtain a lithium ion sieve precursor Li 1.6 R x Mn 1.6-x O4 powder;
[0014] Step 3: Prepare the lithium ion sieve precursor Li1.6 R x Mn 1.6-x The O4 powder is acid-washed, filtered, washed with deionized water and dried to obtain the cation-doped modified lithium ion sieve Li 1.6 R x Mn 1.6-x O4;
[0015] The molecular formula of the cation-doped modified lithium ion sieve is Li 1.6 R x Mn 1.6-x O4, R is selected from at least one of the following: Ti, Fe, Co, Cu, Ni, Zn, Zr, Ce, 0.01≤x≤0.25.
[0016] In the first step, the target doping element salt is selected from Ni(NO3)2·6H2O, Co(NO3)2·6H2O, Cu(NO3)2·6H2O, Zn(NO3)2·6H2O, and FeCl3.
[0017] In the first step, the solvent is selected from ethanol.
[0018] The heating rate during calcination in the first step is 1-10°C / min, preferably 5°C / min.
[0019] The heating rate during calcination in the second step is 1-10°C / min, preferably 5-10°C / min.
[0020] In the third step, the acid is selected from hydrochloric acid, sulfuric acid or nitric acid.
[0021] In the third step, the acid concentration is 0.1-0.5 mol / L, and the soaking time is 24-48 hours.
[0022] Due to the adoption of the above technical solution, the present invention has the following advantages and beneficial effects:
[0023] The preparation method of the cation-doped modified lithium ion sieve provided by the present invention uses cheap raw materials, a simple synthesis method, less waste of lithium salt raw materials, and a low lithium-manganese ratio. The obtained product has high purity and a single crystal phase, which is conducive to industrialization. Compared with the original adsorbent, the adsorbent after cation modification has a high adsorption capacity, a reduced manganese dissolution rate, and a high selectivity for lithium ions.
[0024] The present invention provides a method for preparing a cation-doped modified lithium ion sieve, which is a method for preparing lithium manganese oxides modified by different cation doping by a hydrothermal method, and investigates the effect of cation doping on the adsorption amount of lithium ions in salt lake brine. The cation-doped modified lithium ion sieve provided by the present invention has higher adsorption performance and Mn stability, and can improve the cycle stability of the material.
[0025] The preparation method of the cation-doped modified lithium ion sieve provided by the present invention is different from other doped ion sieves in that the doping process synthesizes uniformly doped lithium manganese oxide by a one-step hydrothermal method. The process route of the present invention is simple, the preparation conditions are mild, the reaction cycle is short, and the doped lithium manganese oxide has higher adsorption performance and stability. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 LiMn in Example 1 1-x Fe x O2 and Li 1.6 Fe x Mn 1.6-x Schematic diagram of the XRD pattern of O4.
[0027] Figure 2 For LiMn in Example 2-5 1-x R x Schematic diagram of the XRD pattern of O2.
[0028] Figure 3 is Li in Example 2-5 1.6 R x Mn 1.6-x Schematic diagram of the XRD pattern of O4.
[0029] Figure 4 The cation-doped lithium ion sieve Li in Example 2 1.6 Ni x Mn 1.6-x Schematic diagram of TEM image of O4.
[0030] Figure 5 LiMn in Example 3 1-x Co x Schematic diagram of the SEM spectrum of O2.
[0031] Figure 6 LiMn in Example 4 1-x Cu x Schematic diagram of the TEM spectrum of O2.
[0032] Figure 7 is Li in Example 2-5 1.6 R x Mn 1.6-x Schematic diagram of the SEM image of O4. DETAILED DESCRIPTION
[0033] In order to explain the present invention more clearly, the present invention is further described below in conjunction with preferred embodiments. It should be understood by those skilled in the art that the following specific description is illustrative rather than restrictive, and should not be used to limit the scope of protection of the present invention.
[0034] The cation-doped modified lithium ion sieve provided by the present invention has a molecular formula of Li 1.6 R x Mn 1.6-x O4, where 0.01≤x≤0.25; cation doping can further reduce the manganese dissolution rate during pickling and increase the adsorption capacity in salt lake brine. The synthesis method is simple, and the introduction of doping ions will not change the original spinel structure and other impurity ions.
[0035] Example 1
[0036] A method for preparing a cation-doped modified lithium ion sieve comprises the following steps:
[0037] Step 1: Mix 15g MnCO3 and 3.15g FeCl3 evenly and calcine at 800℃ for 5h in air atmosphere with a heating rate of 5℃ / min to obtain iron-doped Mn 2-x Fe x O3; in the target doping element salt and manganese salt, the molar ratio of Fe to Mn is 0.15:1.
[0038] 8.55 g Mn 2-x Fe x O3 and 5 g LiOH·H2O were ground and mixed for 2 hours, and the molar ratio of Li to Mn was 1.1:1; the mixture was fully reacted in a reactor at 120°C for 48 hours and dried to obtain 11 g LiMn 1-x Fe x O2 powder;
[0039] Step 2: 5 g of LiMn obtained in the first step 1-x Fe x O2 powder was put into a corundum crucible, and the corundum crucible was placed in a muffle furnace and calcined at 400℃ for 24 hours in an air atmosphere. The heating rate during calcination was 5℃ / min, and then naturally cooled to obtain 5.4 g Li doped spinel lithium ion sieve precursor. 1.6 Fe x Mn 1.6-x O4 (x=0.24) powder.
[0040] Step 3: 0.5 g of the lithium ion sieve precursor Li prepared in step 2 1.6 Fe x Mn 1.6-x The O4 powder was immersed in 100 mL of 0.3 mol / L HCl and subjected to acidification treatment for 36 h. The solution after acidification was filtered, washed three times with deionized water, and then dried at 60° C. to obtain 0.5 g of the cation-doped modified lithium ion sieve.
[0041] The molecular formula of the cation-doped modified lithium ion sieve is Li 1.6 Fe x Mn 1.6-x O4, x=0.24.
[0042] Figure 1 LiMn in Example 1 1-x Fe x O2 and Li 1.6 Fe x Mn 1.6-x Schematic diagram of XRD spectrum of O4. It can be seen from the figure that when the iron doping amount is 15%, it is different from the orthorhombic phase LiMnO2 and Li 1.6 Fe x Mn 1.6-x The standard spectrum of O4 is consistent and has a strong peak intensity, indicating that the iron-doped modified ion sieve has good crystallinity.
[0043] Example 2
[0044] A method for preparing a cation-doped modified lithium ion sieve comprises the following steps:
[0045] Step 1: 2.53 g of the target doping element salt Ni(NO3)2·6H2O was ultrasonically dissolved in 10 mL of ethanol. After it was fully dissolved, 20 g of MnCO3 was slowly poured in and ultrasonicated for 2 hours. The mixture was dried at 60°C for 12 hours and then calcined at 800°C for 5 hours in an air atmosphere. The heating rate during calcination was 5°C / min. 14 g of metal-doped modified Mn was obtained. 2-x Ni x O3; in the target doping element salt and manganese salt, the molar ratio of Ni to Mn is 0.05:1.
[0046] 8.55 g of metal-doped Mn 2-x Ni x O3, 5gLiOH·H2O, grind and mix for 2 hours, Mn 2-x Ni x The molar ratio of Li to Mn in O3 and lithium salt is 1.1:1; the mixture is fully reacted in a reactor at 130°C for 48 hours and centrifuged to obtain 11g LiMn 1-x Ni x O2 powder;
[0047] Step 2: 5g of LiMn obtained in the first step 1-x Ni x O2 powder was put into a corundum crucible, and the corundum crucible was placed in a muffle furnace and calcined at 450℃ for 5 hours in an air atmosphere. The heating rate during calcination was 5℃ / min, and then naturally cooled to obtain a spinel lithium ion sieve precursor 5.3gLi1.6 Ni x Mn 1.6-x O4 (x=0.080) powder.
[0048] Step 3: Prepare the lithium ion sieve precursor 0.1gLi 1.6 Ni 0.08 Mn 1.52 The O4 powder was immersed in 200 mL of 0.5 mol / L sulfuric acid for acid treatment for 24 h to elute the lithium ions in the precursor; the solution after acid treatment was filtered and washed three times with deionized water, and then dried at 60° C. to obtain 0.5 g of the cation-doped modified lithium ion sieve.
[0049] The molecular formula of the cation-doped modified lithium ion sieve is Li 1.6 Ni x Mn 1.6-x O4, x=0.08.
[0050] The XRD spectrum of the product is shown in Figure 2 , 3 As shown, SEM spectrum is shown in Figure 7 As shown in a, TEM spectrum is shown in Figure 4 shown. Figure 2 For LiMn in Example 2-5 1-x R x Schematic diagram of the XRD pattern of O2. Figure 3 is Li in Example 2-5 1.6 R x Mn 1.6-x Schematic diagram of the XRD pattern of O4. Figure 4 The cation-doped lithium ion sieve Li in Example 2 1.6 Ni x Mn 1.6-x Schematic diagram of TEM image of O4. Figure 7 is Li in Example 2-5 1.6 R x Mn 1.6-x Schematic diagram of the SEM image of O4.
[0051] From the XRD diagram, it can be seen that the doping modification does not change the original spinel structure, and the characteristic peaks all correspond to the typical cubic phase Li 1.6 Mn 1.6 O4 spinel structure, Figure 4 The interplanar spacing of the lattice planes shown in the HRTEM image is 0.476 and 0.247 nm, which is consistent with the cubic Li 1.6 Mn 1.6The interplanar spacing of the (111) and (311) lattice planes of O4 is consistent. Due to the shrinkage of the crystal package, the interplanar spacing is slightly reduced after doping, indicating that the material has high crystallinity and exists in the form of polycrystalline. SEM spectrum is shown in Figure 7 As shown in figure a, the particle size of the sample after doping and modification is about 200 nm, the primary particles agglomerated into secondary particles, and the agglomerates are about 4 μm-8 μm.
[0052] Example 3
[0053] A method for preparing a cation-doped modified lithium ion sieve comprises the following steps:
[0054] Step 1: Ultrasonic dissolve the target doping element salt 2.45g Co(NO3)2·6H2O in 10mL ethanol, slowly pour in 20g manganese carbonate after fully dissolved and continue ultrasonication for 2 hours, dry at 60℃ for 12 hours, and then calcine at 800℃ for 5h in air atmosphere, with a heating rate of 5℃ / min, to obtain 14g Mn doped with metal. 2-x Co x O3; in the target doping element salt and manganese salt, the molar ratio of Co to Mn is 0.05:1.
[0055] 8.2 g of metal-doped Mn 2-x Co x O3, 5gLiOH·H2O, grind and mix for 1 hour, Mn 2-x Co x The molar ratio of Li to Mn in O3 and lithium salt is 1.15:1; the mixture is fully reacted in a reactor at 140°C for 60 hours and centrifuged to obtain 11.08 g LiMn 1-x Co x O2 powder;
[0056] Step 2: 2g of LiMn obtained in the first step 1-x Co x O2 powder was put into a corundum crucible, and the corundum crucible was placed in a muffle furnace and calcined at 500℃ for 24 hours in an air atmosphere. The heating rate during calcination was 5℃ / min, and then naturally cooled to obtain a spinel lithium ion sieve precursor 2.2gLi 1.6 Co x Mn 1.6-x O4 (x=0.080) powder.
[0057] Step 3: Prepare the lithium ion sieve precursor 0.1gLi 1.6 Co x Mn 1.6-xThe O4 powder was immersed in 20 mL of 0.1 mol / L nitric acid for 24 h for acidification to elute the lithium ions in the precursor; the solution after acidification was filtered and washed three times with deionized water, and then dried at 60° C. to obtain 0.1 g of the cation-doped modified lithium ion sieve.
[0058] The molecular formula of the cation-doped modified lithium ion sieve is Li 1.6 Co x Mn 1.6-x O4, x=0.08.
[0059] The XRD spectrum of the product is shown in Figure 2 , 3 , intermediate LiMn 1-x Co x The SEM spectrum of O2 is shown in Figure 5 As shown, Figure 5 LiMn in Example 3 1-x Co x Schematic diagram of the SEM spectrum of O2.
[0060] From LiMn 1-x Co x O2 and Li 1.6 Co x Mn 1.6-x The XRD pattern of O4 shows that the doped sample is different from the orthorhombic phase LiMnO2 and Li 1.6 Co x Mn 1.6-x The standard spectrum of O4 is consistent, indicating that the doping modification has not changed the crystal structure of the product and the intermediate and has a strong peak intensity and good crystallinity. Figure 7 As shown in b, morphology analysis shows that the particle size of the sample after doping and modification is about 100-200nm, the primary particles agglomerate into secondary particles, and the agglomerates are about 4μm-8μm.
[0061] Example 4
[0062] A method for preparing a cation-doped modified lithium ion sieve comprises the following steps:
[0063] Step 1: 1.26 g of the target doping element salt Cu(NO3)2·6H2O was ultrasonically dissolved in 30 mL of ethanol. After it was fully dissolved, 41 g of manganese acetate was slowly poured in and ultrasonicated for 2 hours. The mixture was dried at 60°C for 12 hours and then calcined at 800°C for 5 hours in an air atmosphere. The heating rate during calcination was 5°C / min to obtain metal-doped modified Mn 2-x Cu x O3; in the target doping element salt and manganese salt, the molar ratio of Cu to Mn is 0.03:1.
[0064] 8.55 g of metal-doped Mn 2-x Cu x O3, 5gLiOH·H2O, grind and mix for 3 hours, Mn 2-x Cu x The molar ratio of Li to Mn in O3 and lithium salt is 1.1:1; the mixture is fully reacted in a reactor at 140°C for 48 hours and dried to obtain 11g LiMn 1-x Cu x O2 powder;
[0065] Step 2: 3g of LiMn obtained in the first step 1-x Cu x O2 powder was put into a corundum crucible, and the corundum crucible was placed in a muffle furnace and calcined at 500℃ for 5 hours in an air atmosphere. The heating rate during calcination was 10℃ / min, and then naturally cooled to obtain the spinel lithium ion sieve precursor 3.3gLi 1.6 Cu x Mn 1.6-x O4 (x=0.08) powder.
[0066] Step 3: Prepare the lithium ion sieve precursor 0.1gLi 1.6 Cu x Mn 1.6-x The O4 powder was immersed in 60 mL of 0.3 mol / L nitric acid for acidification for 24 h to elute the lithium ions in the precursor; the solution after acidification was filtered and washed three times with deionized water, and then dried at 60° C. to obtain 0.1 g of the cation-doped modified lithium ion sieve.
[0067] The molecular formula of the cation-doped modified lithium ion sieve is Li 1.6 Cu x Mn 1.6-x O4, x=0.08.
[0068] The XRD spectrum of the product is shown in Figure 3 , TEM spectrum see Figure 6 shown. Figure 6 LiMn in Example 4 1-x Cu x Schematic diagram of TEM spectrum of O2. From the XRD diagram, it can be seen that copper doping modification does not lead to the appearance of impurities, and the original spinel structure is still maintained. From the peak shape, it can be seen that the crystallinity of this sample is good. The TEM diagram shows that this sample is a polycrystalline structure. SEM spectrum is shown in Figure 7 Figure c shows that morphology analysis shows that most of the surface particles of the doped and modified samples have a particle size of about 50-200 nm, and the primary particles are agglomerated into secondary particles. It can be seen that the surface is smooth and has a typical octahedral spinel structure.
[0069] Example 5
[0070] A method for preparing a cation-doped modified lithium ion sieve comprises the following steps:
[0071] Step 1: 3.6 g of the target doping element salt Zn(NO3)2·6H2O was ultrasonically dissolved in 15 mL of ethanol. After it was fully dissolved, 20 g of manganese carbonate was slowly poured in and ultrasonicated for 2 hours. The mixture was dried at 60°C for 12 hours and then calcined at 800°C for 5 hours in an air atmosphere. The heating rate during calcination was 5°C / min. 14 g of metal-doped modified Mn 2-x Zn x O3; in the target doping element salt and manganese salt, the molar ratio of Zn to Mn is 0.07:1.
[0072] 5g metal-doped Mn 2-x Zn x O3, 3gLiOH·H2O, grind and mix for 2 hours, Mn 2-x Zn x The molar ratio of Li to Mn in O3 and lithium salt is 1.15:1; the mixture is fully reacted in a reactor at 140°C for 48 hours and centrifuged to obtain 6.04 g LiMn 1-x Zn x O2 powder;
[0073] Step 2: 3g of LiMn obtained in the first step 1-x Zn x O2 powder was put into a corundum crucible, and the corundum crucible was placed in a muffle furnace and calcined at 500℃ for 5 hours in an air atmosphere. The heating rate during calcination was 5℃ / min, and then naturally cooled to obtain a spinel lithium ion sieve precursor 3.27gLi 1.6 Zn x Mn 1.6-x O4 (x=0.112) powder.
[0074] Step 3: Prepare the lithium ion sieve precursor 0.1gLi 1.6 Zn x Mn 1.6-x The O4 powder was immersed in 20 mL of 0.1 mol / L nitric acid for acidification for 24 h to elute the lithium ions in the precursor; the solution after acidification was filtered and washed three times with deionized water, and then dried at 60° C. to obtain 0.5 g of the cation-doped modified lithium ion sieve.
[0075] The molecular formula of the cation-doped modified lithium ion sieve is Li 1.6 Zn x Mn1.6-x O4, x=0.112.
[0076] The XRD spectrum of the product is shown in Figure 3 , SEM spectrum see Figure 7 As shown in Figure d. From the XRD graph, it can be seen that zinc doping modification does not lead to the appearance of impurity phases, and the original spinel structure is still maintained. From the peak shape, it can be seen that this sample has good crystallinity. The SEM image shows that the morphology of this sample is octahedral, and the particle size of the sample after doping modification is about 200nm. The primary particles agglomerate into secondary particles, and the agglomerates are about 5μm-10μm.
[0077] Comparative Example 1
[0078] Compared with Example 1, Comparative Example 1 is different in that no doping element salt is included in the first step.
[0079] 0.5 g of the cation-doped modified lithium ion sieves in Examples 2-5 and Comparative Example 1 were respectively weighed and put into 100 ml of a 25 mmol / L mixed ion solution, placed in a constant temperature shaker, and adsorbed at 25°C for 48 h. The lithium ion sieve was acid-washed (hydrochloric acid time 24 hours), and the ion concentration, manganese dissolution rate, desorption amount and adsorption capacity in the supernatant were measured by ICP. The results are shown in Table 1.
[0080] Table 1 Manganese dissolution rate, desorption amount and adsorption capacity of lithium ion sieves in different embodiments and comparative examples
[0081] Manganese dissolution rate (%) Desorption amount (mg / g) Adsorption capacity (mg / g) Example 1 0.4 61 46 Example 2 0.3 60 47 Example 3 0.1 62 45 Example 4 0.4 65 43 Example 5 0.7 68 44 Comparative Example 1 1.4 58 44
[0082] It can be seen from Table 1 that: (1) compared with the Li before modification in Comparative Example 1 1.6 Mn 1.6 O4, in the cation-doped modified lithium ion sieve prepared by the present invention, R replaces Mn to form a strong bond of R-Mn-O, and increases the adsorption capacity of the lithium ion sieve during the cycle, while improving the adsorption performance and solubility resistance; it shows that the cation-doped modified lithium ion sieve prepared by the present invention has the advantages of high adsorption capacity, high selectivity and low manganese dissolution rate.
[0083] (2) The cation-doped modified lithium ion sieve prepared by the method of the present invention is pickled, and then lithium ions are adsorbed by salt lake brine. Combined with the data in Table 1 above, it can be seen that the manganese dissolution rate of the cation-doped modified lithium ion sieve in Examples 1-5 is 0.4%, 0.3%, 0.1%, 0.4%, and 0.7%, respectively, and the desorption amount is 61, 60, 62, 65, and 68 mg / g, respectively, and the adsorption amount is 46, 47, 45, 43, and 44 mg / g, respectively; while the manganese dissolution rate of the lithium ion sieve in Comparative Example 1 is 1.4%, the desorption amount is 58 mg / g, and the adsorption amount is 44 mg / g. The results show that cation doping effectively improves the stability of the adsorbent, reduces the manganese dissolution rate, and increases the adsorption amount. The method of the present invention is conducive to large-scale production and application in actual brine lithium extraction projects.
[0084] Comparative Example 2
[0085] Example 7 of the patent application with publication number CN103991908A is used as comparative example 2.
[0086] Dissolve 80.0mmol lithium nitrate in 20ml deionized water, then add 98.0mmol manganese carbonate and 1.0mmol cobalt trioxide. Stir in a water bath at 80℃ and evaporate to dryness. Transfer the resulting mixture to a muffle furnace and calcine at 450℃ for 24 hours. After cooling, elute in 1mol / l ammonium persulfate solution to obtain ion sieve Mn 0.98 Co 0.02 O2·0.31H2O, the manganese dissolution rate during the pickling process is only 0.7%.
[0087] Compared with Comparative Example 2, the method of the present invention has a lower manganese dissolution rate (the manganese dissolution rate of Comparative Example 2 is 0.7%, and the manganese dissolution rate of the present invention is 0.1%) and the adsorption and desorption amount is improved. Reducing the manganese dissolution rate is the key to manganese-based adsorbents. By reducing the manganese dissolution rate, the stability can be improved, thereby increasing the number of uses and application value of the adsorbent.
[0088] The above is only a preferred embodiment of the present invention, and does not limit the present invention in any form. Although the present invention has been disclosed as a preferred embodiment, it is not used to limit the present invention. Any technician familiar with this patent can make some changes or modify the technical contents suggested above into equivalent embodiments without departing from the scope of the technical solution of the present invention. However, any simple modification, equivalent change and modification made to the above embodiments according to the technical essence of the present invention without departing from the content of the technical solution of the present invention still fall within the scope of the solution of the present invention.
Claims
1. A method for preparing a cation-doped modified lithium ion sieve, characterized in that: The following steps are involved: Step 1: ultrasonically dissolve the target doping element salt in the solvent, slowly pour in the manganese salt after it is fully dissolved and continue ultrasonication for 1 to 5 hours, dry at 50 to 80 ° C for 1 to 12 hours, and then calcine at 500 to 800 ° C for 3 to 12 hours in an air atmosphere to obtain metal-doped modified Mn 2-x R x O3; Alternatively, the target doping element salt and the manganese salt are mixed evenly, and calcined at 500-800°C for 3-12 hours in an air atmosphere to obtain a metal-doped modified Mn 2-x R x O3; In the target doping element salt and manganese salt, the molar ratio of R to Mn is (0.01-0.18):1; Metal doped modified Mn 2-x R x O3, lithium salt grinding and mixing, Mn 2-x R x The molar ratio of Li to Mn in O3 and lithium salt is (1-1.2):1; fully react at a temperature of 100-180°C for 1-72 hours, and dry to obtain LiMn 1-x R x O2 powder; The manganese salt is selected from at least one of manganese acetate, manganese carbonate, manganese sulfate and manganese iodide; The lithium salt is selected from at least one of LiOH·H2O, LiNO3 or Li2CO3; Step 2: LiMn obtained in the first step 1-x R x The O2 powder is calcined at 300-500°C in an air atmosphere for 4-72 hours to obtain a lithium ion sieve precursor Li 1.6 R x Mn 1.6-x O4 powder; Step 3: Prepare the lithium ion sieve precursor Li 1.6 R x Mn 1.6-x The O4 powder is acid-washed, filtered, washed with deionized water and dried to obtain the cation-doped modified lithium ion sieve Li 1.6 R x Mn 1.6-x O4; The molecular formula of the cation-doped modified lithium ion sieve is Li 1.6 R x Mn 1.6-x O4, R is selected from at least one of the following: Ti, Fe, Co, Cu, Ni, Zn, Zr, Ce, 0.01≤x≤0.25; In the first step, the target doping element salt is selected from Ni(NO3)2·6H2O, Co(NO3)2·6H2O, Cu(NO3)2·6H2O, Zn(NO3)2·6H2O, and FeCl3; In the first step, the solvent is selected from ethanol; In the third step, the acid is selected from hydrochloric acid, sulfuric acid or nitric acid; In the third step, the acid concentration is 0.1-0.5 mol / L, and the soaking time is 24-48 hours.
2. The method for preparing the cation-doped modified lithium ion sieve according to claim 1, characterized in that: The heating rate during calcination in the first step is 1-10°C / min.
3. The method for preparing the cation-doped modified lithium ion sieve according to claim 1, characterized in that: The heating rate during calcination in the second step is 1-10°C / min.