A preparation method and application of light hydrocarbon cracking catalyst

The light hydrocarbon catalyst is prepared by using a compound of low silicon to aluminum ratio ZSM-5 and high silicon to aluminum ratio ZSM-5 molecular sieves, which solves the problems of cumbersome catalyst process and insufficient yield of low carbon olefins, and achieves high selectivity and stability. The process is simplified to meet part of the growth in market demand for propylene.

CN116371454BActive Publication Date: 2024-10-01SHANDONG CHAMBROAD PETROCHEMICALS CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202310365233.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-04-07
Publication Date
2024-10-01
Estimated Expiration
2043-04-07

AI Technical Summary

Technical Problem

The catalyst preparation process in the existing technology is cumbersome and difficult to achieve industrial application, and the traditional steam thermal cracking method cannot meet the market demand for propylene, resulting in insufficient low-carbon olefin yield and selectivity.

Method used

Using a compound of low silicon to aluminum ratio ZSM-5 and high silicon to aluminum ratio ZSM-5 molecular sieves, deoxygenated ionized water, low silicon to aluminum ratio ZSM-5, kaolin, aluminum sol, pseudo-boehmite and phosphorus precursors Mixing and acidification treatment, ball milling and granulation are carried out to form a microsphere particle catalyst, and the light hydrocarbon cracking catalyst is obtained by molding, drying and roasting through high-temperature spray centrifugal equipment.

Benefits of technology

The light hydrocarbon catalytic cracking catalyst achieves the effects of high low-carbon olefin yield, good selectivity and good stability, simplifies the preparation process, is easy for industrial application, and improves the yields of propylene and ethylene.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004166427530000051
    Figure BDA0004166427530000051
  • Figure BDA0004166427530000061
    Figure BDA0004166427530000061
  • Figure BDA0004166427530000062
    Figure BDA0004166427530000062
Patent Text Reader

Abstract

The present invention provides a preparation method and application of a light hydrocarbon cracking catalyst, comprising the following steps: uniformly mixing deoxygenated ionized water, a low silicon-aluminum ratio ZSM-5 molecular sieve and a high silicon-aluminum ratio ZSM-5 molecular sieve to obtain slurry A; uniformly mixing deoxygenated ionized water, kaolin and aluminum sol to obtain slurry B; uniformly mixing the slurry B and pseudo-boehmite to obtain slurry C; acidifying the slurry C to obtain slurry D; mixing the slurry D and a precursor of phosphorus to obtain slurry E; granulating the slurry E after ball milling to obtain microsphere particles; drying and burning the microsphere particles to obtain a light hydrocarbon cracking catalyst. The present invention adopts a compound of a low silicon-aluminum ratio ZSM-5 molecular sieve and a high silicon-aluminum ratio ZSM-5 molecular sieve, so that the prepared catalyst has a high yield of low-carbon olefins, good selectivity, good stability, and is easy to industrialize and apply when used for naphtha cracking.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of petroleum catalytic cracking, and in particular relates to a preparation method of a light hydrocarbon cracking catalyst and application thereof. Background Art

[0002] As important basic raw materials in the petrochemical industry, ethylene and propylene are traditionally produced mainly through tubular furnace steam cracking. Cracking raw materials include naphtha, light diesel, ethane and liquefied petroleum gas. However, with the sharp increase in demand for olefin derivatives, the propylene output obtained by thermal cracking can no longer meet the growing demand for propylene in the domestic and foreign markets. At the same time, the steam thermal cracking method itself has many shortcomings. Therefore, on the basis of optimizing the allocation of cracking raw material resources, the use of new processes and technologies to replace traditional steam thermal cracking technology for producing low-carbon olefins has become an inevitable trend in the development of this field. Light hydrocarbon catalytic cracking and other processes have gradually emerged and developed in recent years, which has alleviated the market demand for propylene to a certain extent.

[0003] For oil refining companies, due to the rise of large-scale integrated refining and chemical companies, there is a great surplus of refining capacity, resulting in an oversupply of oil products in the market. Therefore, it has become an inevitable trend to convert low-value-added oil products into high-value-added chemicals or chemical intermediates. Catalytic cracking of light hydrocarbons to produce low-carbon olefins is a process technology with great market prospects. It can crack C10 or less alkanes, olefins, and cycloalkanes into ethylene, propylene, and BTX under the action of catalysts, which can reduce gasoline production to a certain extent, convert it into high-value-added low-carbon olefin resources, and increase corporate profitability.

[0004] The hotspot and difficulty in the field of catalytic cracking technology is the research and preparation of catalysts. However, the existing technology for preparing catalysts is complicated and difficult to achieve industrial application. Summary of the invention

[0005] In view of this, the object of the present invention is to provide a method for preparing a light hydrocarbon cracking catalyst and its application. The method is simple, and the light hydrocarbon catalytic cracking catalyst has the advantages of high yield of low-carbon olefins, good selectivity, and easy industrial application.

[0006] The present invention provides a method for preparing a light hydrocarbon cracking catalyst, comprising the following steps:

[0007] The deoxygenated ionized water, the low silicon-aluminum ratio ZSM-5 molecular sieve and the high silicon-aluminum ratio ZSM-5 molecular sieve are uniformly mixed to obtain slurry A;

[0008] Mix deoxygenated ionized water, kaolin and aluminum sol and add to the slurry A to obtain slurry B;

[0009] The slurry B and pseudo-boehmite are mixed evenly to obtain slurry C;

[0010] Acidifying the slurry C to obtain slurry D;

[0011] Mixing the slurry D with a phosphorus precursor to obtain slurry E;

[0012] The slurry E is ball-milled and granulated to obtain microsphere particles;

[0013] The microsphere particles are dried and burned to obtain a light hydrocarbon cracking catalyst.

[0014] In the present invention, the molar ratio of Si:Al in the low silicon-aluminum ratio ZSM-5 molecular sieve is 20 to 50; the molar ratio of Si:Al in the high silicon-aluminum ratio ZSM-5 molecular sieve is 60 to 150. In a specific embodiment, the molar ratio of Si:Al in the low silicon-aluminum ratio ZSM-5 molecular sieve is 25; the molar ratio of Si:Al in the high silicon-aluminum ratio ZSM-5 molecular sieve is 110.

[0015] The ZSM-5 molecular sieve used in the present invention has a special MFI pore structure, adjustable acid properties, and good thermal stability. In the present invention, a low silicon-aluminum ratio ZSM-5 molecular sieve and a high silicon-aluminum ratio ZSM-5 molecular sieve are compounded, so that the prepared catalyst has the advantages of high light olefin yield, high selectivity, and good stability when used in light hydrocarbon cracking reactions.

[0016] In the present invention, the mass ratio of the total amount of deoxygenated ionized water, the total amount of molecular sieve, kaolin, aluminum sol, pseudo-boehmite and hydrochloric acid is (30-70):(5-40):(3-20):(3-30):(1-10):(0.5-8).

[0017] The present invention preferably uses hydrochloric acid for acidification, wherein the mass concentration of the hydrochloric acid is 35% to 37%, and the acidification time is 50 to 80 minutes.

[0018] In the present invention, the phosphorus precursor is selected from one or more of phosphoric acid, ammonium dihydrogen phosphate and diammonium hydrogen phosphate; the mass proportion of the phosphorus precursor in the slurry D is 0.5-8%.

[0019] The present invention adopts a high-temperature spray centrifugal device to shape the slurry D after ball milling to obtain microsphere particles. The particle size of the microsphere particles is 20 to 150 μm.

[0020] In the present invention, the drying temperature is 100-130° C., and the drying time is 5-8 hours; the roasting temperature is 450-550° C., and the roasting time is 3-6 hours.

[0021] The present invention provides an application of a light hydrocarbon cracking catalyst prepared by the preparation method described in the above technical scheme in naphtha cracking.

[0022] The present invention provides a preparation method of a light hydrocarbon cracking catalyst, comprising the following steps: uniformly mixing deoxygenated ionized water, a low silicon-aluminum ratio ZSM-5 molecular sieve and a high silicon-aluminum ratio ZSM-5 molecular sieve to obtain slurry A; uniformly mixing deoxygenated ionized water, kaolin and aluminum sol and adding the mixture to the slurry A to obtain slurry B; uniformly mixing the slurry B and pseudo-boehmite to obtain slurry C; acidifying the slurry C to obtain slurry D; mixing the slurry D and a phosphorus precursor to obtain slurry E; ball-milling the slurry E and granulating it to obtain microsphere particles; drying and burning the microsphere particles to obtain a light hydrocarbon cracking catalyst. The present invention adopts a compound of a low silicon-aluminum ratio ZSM-5 molecular sieve and a high silicon-aluminum ratio ZSM-5 molecular sieve, so that the prepared catalyst has a high yield of low-carbon olefins, good selectivity, good stability, and is easy to industrialize and apply when used for naphtha cracking. DETAILED DESCRIPTION

[0023] In order to further illustrate the present invention, the preparation method and application of a light hydrocarbon cracking catalyst provided by the present invention are described in detail below in combination with examples, but they should not be construed as limiting the scope of protection of the present invention.

[0024] Example 1

[0025] (1) Add 150 g of low silicon-aluminum ratio ZSM-5 (SiO2 / Al2O3=25) molecular sieve and 150 g of high silicon-aluminum ratio ZSM-5 (SiO2 / Al2O3=110) molecular sieve to 1000 g of deionized water, and mix them in a ball mill to obtain slurry A;

[0026] (2) adding 220 g of kaolin and 320 g of aluminum sol to deionized water, stirring evenly, adding slurry A, mixing and slurrying to obtain slurry B;

[0027] (3) Add 100 g of pseudo-boehmite to slurry B and stir evenly to obtain slurry C;

[0028] (4) Add 30 g of hydrochloric acid to slurry C for acidification and stir evenly to obtain slurry D;

[0029] (5) Add 30 g of diammonium phosphate to slurry D and stir evenly to obtain slurry E;

[0030] (6) The slurry E is ball-milled by a ball mill, and the ball-milled slurry is molded by a high-temperature spray centrifugal device to obtain microsphere particles with a particle size of 20 to 150 μm;

[0031] (7) The microsphere catalyst was dried at 120°C for 3 h and calcined at 540°C for 4 h. The calcined catalyst was evaluated using a riser.

[0032] Example 2

[0033] (1) Add 100 g of low silicon-aluminum ratio ZSM-5 (SiO2 / Al2O3=25) molecular sieve and 200 g of high silicon-aluminum ratio ZSM-5 (SiO2 / Al2O3=110) molecular sieve to 1000 g of deionized water, and mix them in a ball mill to obtain slurry A;

[0034] (2) adding 220 g of kaolin and 320 g of aluminum sol to deionized water, stirring evenly, adding slurry A, mixing and beating to obtain slurry B;

[0035] (3) Add 100 g of pseudo-boehmite to slurry B and stir evenly to obtain slurry C;

[0036] (4) Add 30 g of hydrochloric acid to slurry C for acidification and stir evenly to obtain slurry D;

[0037] (5) Add 28 g of ammonium dihydrogen phosphate to slurry D and stir evenly to obtain slurry E;

[0038] (6) The slurry E is ball-milled by a ball mill, and the ball-milled slurry is molded by a high-temperature spray centrifugal device to obtain microsphere particles with a particle size of 20 to 150 μm;

[0039] (7) The microsphere catalyst was dried at 120°C for 3 h and calcined at 540°C for 4 h. The calcined catalyst was evaluated using a riser.

[0040] Example 3

[0041] (1) Add 200 g of low silicon-aluminum ratio ZSM-5 (SiO2 / Al2O3=25) molecular sieve and 100 g of high silicon-aluminum ratio ZSM-5 (SiO2 / Al2O3=110) molecular sieve to 1000 g of deionized water, and mix them in a ball mill to obtain slurry A;

[0042] (2) adding 220 g of kaolin and 320 g of aluminum sol to deionized water, stirring evenly, adding slurry A, mixing and beating to obtain slurry B;

[0043] (3) Add 100 g of pseudo-boehmite to slurry B and stir evenly to obtain slurry C;

[0044] (4) Add 30 g of hydrochloric acid to slurry C for acidification and stir evenly to obtain slurry D;

[0045] (5) Add 35 g of ammonium dihydrogen phosphate to slurry D and stir evenly to obtain slurry E;

[0046] (6) The slurry E is ball-milled by a ball mill, and the ball-milled slurry is molded by a high-temperature spray centrifugal device to obtain microsphere particles with a particle size of 20 to 150 μm;

[0047] (7) The microsphere catalyst was dried at 120°C for 3 h and calcined at 540°C for 4 h. The calcined catalyst was evaluated using a riser.

[0048] Comparative Example 1

[0049] (1) adding 300 g of high silicon-aluminum ratio ZSM-5 (SiO2 / Al2O3=110) molecular sieve to 1000 g of deionized water, and milling and mixing in a ball mill to obtain slurry A;

[0050] (2) adding 220 g of kaolin and 320 g of aluminum sol to deionized water, stirring evenly, adding slurry A, mixing and slurrying to obtain slurry B;

[0051] (3) Add 100 g of pseudo-boehmite to slurry B and stir evenly to obtain slurry C;

[0052] (4) Add 30 g of hydrochloric acid to slurry C for acidification and stir evenly to obtain slurry D;

[0053] (5) Add 25 g of ammonium dihydrogen phosphate to slurry D and stir evenly to obtain slurry E;

[0054] (6) The slurry E is ball-milled by a ball mill, and the ball-milled slurry is molded by a high-temperature spray centrifugal device to obtain microsphere particles with a particle size of 20 to 150 μm;

[0055] (7) The microsphere catalyst was dried at 120°C for 3 h and calcined at 540°C for 4 h. The calcined catalyst was evaluated using a riser.

[0056] Comparative Example 2

[0057] (1) adding 300 g of low silicon-aluminum ratio ZSM-5 (SiO2 / Al2O3=25) molecular sieve to 500 g of deionized water, and milling and mixing in a ball mill to obtain slurry A;

[0058] (2) adding 220 g of kaolin and 320 g of aluminum sol to deionized water, stirring evenly, adding slurry A, mixing and slurrying to obtain slurry B;

[0059] (3) Add 100 g of pseudo-boehmite to slurry B and stir evenly to obtain slurry C;

[0060] (4) Add 30 g of hydrochloric acid to slurry C for acidification and stir evenly to obtain slurry D;

[0061] (5) Add 35 g of ammonium dihydrogen phosphate to slurry D and stir evenly to obtain slurry E;

[0062] (6) The slurry E is ball-milled by a ball mill, and the ball-milled slurry is molded by a high-temperature spray centrifugal device to obtain microsphere particles with a particle size of 20 to 150 μm;

[0063] (7) The microsphere catalyst was dried at 120°C for 3 h and calcined at 540°C for 4 h. The calcined catalyst was evaluated using a riser.

[0064] The evaluation conditions for the pilot riser are:

[0065] Table 1 Evaluation conditions

[0066]

[0067] Table 2 Naphtha raw material properties

[0068]

[0069] Table 3 Product properties

[0070]

[0071] As can be seen from the above embodiments, the present invention provides a method for preparing a light hydrocarbon cracking catalyst, comprising the following steps: uniformly mixing deoxygenated ionized water, a low silicon-aluminum ratio ZSM-5 molecular sieve and a high silicon-aluminum ratio ZSM-5 molecular sieve to obtain slurry A; mixing deoxygenated ionized water, kaolin and aluminum sol and adding them to the slurry A to obtain slurry B; uniformly mixing the slurry B and pseudo-boehmite to obtain slurry C; acidifying the slurry C to obtain slurry D; mixing the slurry D with a phosphorus precursor to obtain slurry E; ball-milling the slurry E and granulating it to obtain microsphere particles; drying and burning the microsphere particles to obtain a light hydrocarbon cracking catalyst. The present invention adopts a compound of a low silicon-aluminum ratio ZSM-5 molecular sieve and a high silicon-aluminum ratio ZSM-5 molecular sieve, so that the prepared catalyst has a high yield of low-carbon olefins, good selectivity, good stability, and is easy to industrialize when used for naphtha cracking. The experimental results show that the yield of ethylene is 19.65-21.03%, and the yield of propylene is 21.64-23.63%.

[0072] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. Application of a light hydrocarbon cracking catalyst in naphtha cracking; The preparation method of the light hydrocarbon cracking catalyst, The following steps are involved: Deoxygenated ionized water, a low silicon-aluminum ratio ZSM-5 molecular sieve and a high silicon-aluminum ratio ZSM-5 molecular sieve are uniformly mixed to obtain slurry A; the molar ratio of Si:Al in the low silicon-aluminum ratio ZSM-5 molecular sieve is 20-50; the molar ratio of Si:Al in the high silicon-aluminum ratio ZSM-5 molecular sieve is 60-150; the mass ratio of the low silicon-aluminum ratio ZSM-5 molecular sieve to the high silicon-aluminum ratio ZSM-5 molecular sieve is 0.1:1-10:1; Mixing deoxygenated ionized water, kaolin and aluminum sol and adding the mixture to the slurry A to obtain slurry B; The slurry B and pseudo-boehmite are mixed evenly to obtain slurry C; Adding hydrochloric acid to the slurry C for acidification to obtain slurry D; The slurry D and a phosphorus precursor are mixed to obtain a slurry E; the phosphorus precursor is selected from one or more of diammonium phosphate and diammonium hydrogen phosphate; the phosphorus precursor accounts for 0.5-8% of the mass of the slurry D; The slurry E is ball-milled and granulated to obtain microsphere particles; Drying and calcining the microsphere particles to obtain a light hydrocarbon cracking catalyst; The mass ratio of the total amount of deoxygenated ionized water, the total amount of molecular sieve, kaolin, aluminum sol, pseudo-boehmite and hydrochloric acid is (30-70): (5-40): (3-20): (3-30): (1-10): (0.5-8).

2. The use according to claim 1, It is characterized in that The granulation is carried out by spray centrifugation.

3. The use according to claim 1, It is characterized in that The drying temperature is 100-130°C and the drying time is 5-8h; The calcination temperature is 450-550° C., and the calcination time is 3-6 hours.

4. The use according to claim 1, It is characterized in that The particle size of the microsphere particles is 20-150 μm.

Citation Information

Patent Citations

  • ZSM-5 molecular sieve catalyst for preparing propylene by conversion of methanol and preparation method thereof

    CN101940942A

  • Fluidized bed catalyst for preparing alkene through catalytic cracking

    CN102371172A

  • Method for preparing ethylene and propylene through catalytic cracking of light hydrocarbons

    CN102746873A

  • Fluidized-bed catalyst for preparing arene and propylene from oxygenated compound and application of fluidized-bed catalyst

    CN106607074A

  • Preparation method and application of catalyst for preparing low-carbon olefin through catalytic cracking of straight-run diesel oil

    CN115624987A