A biomass-based emulsifier for waterborne epoxy anticorrosive coating resin and preparation method thereof

By grafting sodium lignosulfonate with polyethylene glycol monomethyl ether and combining it with bisphenol A epoxy resin, a biomass-based emulsifier with anionic and nonionic hydrophilic groups is formed, which solves the problem of water-based epoxy resin in Stability issues in acid, metal salt, and hard water environments improve the emulsification effect and anti-corrosion performance of coatings, achieving effective water-based epoxy resin and high-value utilization of waste crops.

CN116376032BActive Publication Date: 2024-10-11LUDONG UNIVERSITY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211717928.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-30
Publication Date
2024-10-11
Estimated Expiration
2042-12-30

AI Technical Summary

Technical Problem

Existing water-based epoxy resin emulsifiers lose their stability in environments such as acids, metal salts, and hard water, and have insufficient emulsifying ability to effectively dissolve epoxy resin, making it difficult to achieve water-based epoxy resins.

Method used

By grafting sodium lignosulfonate with polyethylene glycol monomethyl ether, a biomass-based emulsifier with anionic hydrophilic groups and nonionic hydrophilic groups is formed, combined with bisphenol A epoxy resin, to improve the emulsifier emulsifying effect and stability.

Benefits of technology

It achieves stable emulsification in environments such as acids, metal salts, and hard water, improves the emulsification effect of the emulsifier, reduces production costs, increases the added value of waste crops, and prepares water-based epoxy coatings with excellent anti-corrosion properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 221230162351
    Figure 221230162351
Patent Text Reader

Abstract

The invention discloses a biomass-based emulsifier for waterborne epoxy anticorrosive coating resin and a preparation method thereof: lignin, sodium hydride and dimethyl sulfoxide from abandoned crops are placed at room temperature for reaction for 30 min, 1,3-propane sultone is added, the temperature is raised to 60-80 ° C with stirring, the reactor is evacuated and filled with nitrogen three times, and the reaction is performed for 12-16 h to obtain sodium lignin sulfonate. Polyethylene glycol monomethyl ether, sodium hydride and dimethyl sulfoxide are placed at room temperature for reaction for 30 min, and then sodium lignin sulfonate is added to a container, the temperature is raised to 100-120 ° C, evacuated and filled with nitrogen are repeated three times, and the reaction is performed for 12-16 h to obtain sodium lignin sulfonate-polyethylene glycol monomethyl ether. Finally, sodium lignin sulfonate-polyethylene glycol monomethyl ether, sodium hydride, and ethylene glycol propyl ether were placed in a container and reacted at room temperature for 30 min. Bisphenol A epoxy resin was added, and the temperature was raised to 80-100 °C. Vacuuming and nitrogen filling were repeated three times, and the reaction lasted for 16-20 h. The product was cooled to room temperature and discharged to obtain a light yellow transparent lignin epoxy emulsifier.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of emulsifiers, and in particular to a biomass-based emulsifier for waterborne epoxy anticorrosive coating resin and a preparation method thereof. Background Art

[0002] Epoxy resin is a polymer resin with corrosion resistance, good adhesion and high mechanical strength. However, pure epoxy resin is difficult to dissolve in water, but it is easily soluble in some traditional organic solvents. Traditional organic solvents are volatile, so they will cause high VOC and pollute the environment. Therefore, water-based epoxy resin is becoming more and more popular. At present, the method for preparing water-based epoxy resin is mainly to add emulsifiers. Common emulsifiers include non-ionic emulsifiers, anionic emulsifiers, cationic emulsifiers, and amphoteric emulsifiers, among which anionic emulsifiers and non-ionic emulsifiers are more common. Anionic emulsifier systems are relatively stable in alkaline solutions, but they will lose stability when encountering acids, metal salts, and hard water, and will precipitate as gels below the three-phase equilibrium point and lose their emulsifying ability. Nonionic emulsifiers are insensitive to pH changes and are relatively stable; but their emulsifying ability is not as good as that of anionic types. They are generally not used alone, and are often used in combination with anionic emulsifiers to improve the sensitivity of pure anionic emulsification systems to pH values, electrolytes, etc. Nonionic emulsifiers do not have a three-phase equilibrium point, but have a cloud point (the temperature at which the nonionic emulsion system begins to separate as the temperature rises). Above the cloud point, its emulsification ability tends to decrease. To solve the above problems, it is of great significance to design and create an emulsifier that contains both anionic groups and nonionic groups.

[0003] Lignin is a natural high molecular polymer second only to cellulose and chitin in nature, and its source is wide. Extracting lignin from waste crops can increase the added value of waste and reduce the cost of material production. Sodium lignin sulfonate, as a derivative of lignin, is a highly hydrophilic high molecular polymer with anionic hydrophilic groups. In order to improve the emulsification effect of biomass-based emulsifiers, sodium lignin sulfonate is grafted with non-ionic hydrophilic groups (polyethylene glycol monomethyl ether). On the one hand, it solves the problem that sodium lignin sulfonate cannot be emulsified in acid, metal salt, hard water and other environments. On the other hand, the emulsifier has both anionic hydrophilic groups and non-ionic hydrophilic groups, which can greatly improve the emulsification effect of the emulsifier. Therefore, the preparation of biomass-based emulsifiers can not only realize the high-value utilization of waste crops, but also prepare epoxy coatings with excellent anti-corrosion properties, which has important environmental and economic benefits. Summary of the invention

[0004] The present application provides a biomass-based emulsifier for waterborne epoxy anticorrosive coating resin and a preparation method thereof, which on the one hand increases the added value of waste crops, and on the other hand solves the deficiencies in the performance and application technology of anionic emulsifiers and nonionic emulsifiers.

[0005] The technical solution adopted by the present invention to solve the above problems is: a biomass-based emulsifier for water-based epoxy anticorrosive coating resin and a preparation method thereof, characterized by comprising the following steps:

[0006] (1) Lignin extraction method: Crush corn stalks into stalk powder using a crusher. Weigh 100 parts of corn stalk powder and 100-120 parts of ethylene glycol and place them in a hydrothermal reactor. Heat to 180-200 °C for 6-8 hours. After the reaction is completed, cool to room temperature. Filter the product after the reaction under reduced pressure, wash the product with ethylene glycol three times, separate the stalk residue from the lignin solution by centrifugation, add a large amount of water to the lignin solution and stir, precipitate the lignin, freeze-dry the obtained lignin, and obtain brown powder lignin.

[0007] (2) 10-12 parts of purified lignin, 1-3 parts of sodium hydride, and 10-16 parts of dimethyl sulfoxide were placed in a container and reacted at room temperature for 30 min. Then, 2-6 parts of 1,3-propane sultone were added, the temperature was raised to 60-80 °C, and the reactor was evacuated and filled with nitrogen three times. The reaction was repeated for 12-16 h to obtain the product sodium lignin sulfonate solution. Sodium lignin sulfonate powder was prepared by vacuum distillation and freeze drying.

[0008] (3) Add 3-5 parts of polyethylene glycol monomethyl ether, 1-3 parts of sodium hydride, and 10-12 parts of dimethyl sulfoxide to a container, react at room temperature for 30 min, then add 8-10 parts of sodium lignin sulfonate, raise the temperature to 100-120 °C under magnetic stirring, evacuate the reactor and fill it with nitrogen three times, and react for 12-16 h. After the reaction is completed, dimethyl sulfoxide is removed by vacuum distillation to obtain sodium lignin sulfonate-polyethylene glycol monomethyl ether.

[0009] (4) Weigh 16-18 parts of sodium lignin sulfonate-polyethylene glycol monomethyl ether, 1-3 parts of sodium hydride, and 10-12 parts of ethylene glycol propyl ether into a container and react at room temperature for 30 min. Then add 9-11 parts of bisphenol A epoxy resin and raise the temperature to 80-100 °C. React for 16-20 h. Evacuate the reactor and fill it with nitrogen three times. Cool it to room temperature and discharge the material to obtain a light yellow transparent biomass-based epoxy emulsifier.

[0010] The lignin of the present invention is extracted from one of the waste crops such as wheat straw, corn straw, cotton straw, etc.;

[0011] The solvent is any one of ethylene glycol propyl ether, ethylene glycol methyl ether, ethylene glycol ethyl ether, propylene glycol methyl ether, propylene glycol ethyl ether, and propylene glycol propyl ether, or a mixture of any two or more thereof; the polyethylene glycol monomethyl ether is any one of polyethylene glycol monomethyl ether M750, polyethylene glycol monomethyl ether M2000, and polyethylene glycol monomethyl ether M5000, or a mixture of any two or more thereof; the bisphenol A epoxy resin is any one of bisphenol A epoxy resin E20, bisphenol A epoxy resin E44, and bisphenol A epoxy resin E51, or a mixture of any two or more thereof.

[0012] Compared with the prior art, the present invention has the following advantages:

[0013] (1) The raw materials are extracted from corn stalk waste, which not only reduces the production cost but also increases the added value of the waste, with significant environmental and economic benefits.

[0014] (2) Sodium lignin sulfonate with extremely strong hydrophilicity is prepared by modifying lignin. Sodium lignin sulfonate is used as the anionic hydrophilic group and polyethylene glycol monomethyl ether is used as the nonionic hydrophilic group. On the one hand, the problem that sodium lignin sulfonate cannot be emulsified in environments such as acid, metal salt, and hard water is solved. On the other hand, the presence of both anionic hydrophilic groups and nonionic hydrophilic groups can greatly improve the emulsification effect of the emulsifier.

[0015] (3) The lipophilic end is composed of bisphenol A epoxy resin, which is a linear lipophilic structure. Its structure is highly similar to the emulsified oil phase-epoxy resin structure, which enables the emulsifier to better bond to the epoxy resin.

[0016] (4) By introducing linear hydrophilic groups and linear lipophilic groups, the binding ability of the hydrophobic ends in the emulsifier micelles is weakened, so that the emulsifier can be more evenly distributed in the water phase, thereby improving the stability of the emulsion. DETAILED DESCRIPTION

[0017] The present invention will be further described below in conjunction with embodiments:

[0018] Example 1

[0019] The corn stalks were crushed into stalk powder using a crusher. 10 g corn stalk powder and 10 g ethylene glycol were weighed and placed in a hydrothermal reactor, heated to 180 °C for 6 h. After the reaction was completed, the temperature was cooled to room temperature. The product after the reaction was filtered under reduced pressure, and then washed with ethylene glycol for 3 times. The stalk residue and lignin solution were separated by centrifugation. A large amount of water was added to the lignin solution and stirred. The lignin precipitated and the obtained lignin was freeze-dried to obtain brown powder lignin.

[0020] 5 g of purified lignin, 1 g of sodium hydride, and 10 g of dimethyl sulfoxide were placed in a container and reacted at room temperature for 30 min. Then, 1 g of 1,3-propane sultone was added, the temperature was raised to 60 °C, and the reactor was evacuated and filled with nitrogen three times. The reaction was repeated for 12 h to obtain the product sodium lignin sulfonate solution. Sodium lignin sulfonate powder was prepared by vacuum distillation and freeze drying.

[0021] Add 3 g of polyethylene glycol monomethyl ether, 1 g of sodium hydride, and 10 g of dimethyl sulfoxide to the container, react at room temperature for 30 min, then add 8 g of sodium lignin sulfonate, and heat to 100 °C under magnetic stirring. Repeat the vacuum and nitrogen filling of the reactor three times and react for 12 h. After the reaction is completed, dimethyl sulfoxide is removed by vacuum distillation to obtain sodium lignin sulfonate-polyethylene glycol monomethyl ether.

[0022] Weigh 16 g of sodium lignin sulfonate-polyethylene glycol monomethyl ether and 1 g of sodium hydride in a container, use 10 g of ethylene glycol propyl ether as a solvent, react at room temperature for 30 min, then add 9 g of bisphenol A epoxy resin E51, raise the temperature to 80 °C, react for 16 h, evacuate the reactor and fill it with nitrogen three times, cool it to room temperature and discharge it to obtain a light yellow transparent biomass-based epoxy emulsifier.

[0023] Add 1.5 g of lignin emulsifier and 12.5 g of epoxy resin E-44 into a three-necked flask, and install a mechanical stirring paddle, a constant pressure funnel, and a condenser into the three-necked flask. Under stirring conditions, heat to 80 °C and preheat for 2 h. After preheating, lower the temperature to 60 °C, add 11 g of distilled water to the constant pressure dropping funnel, and increase the speed to 3000 r / min. Distilled water is slowly added dropwise into the reaction system, and the viscosity of the epoxy resin increases first and then decreases, that is, the phase inversion process. When all the deionized water is added dropwise, continue to slowly stir and keep warm for 1 h to obtain a milky water-based epoxy resin emulsion with a solid content of 55%.

[0024] The waterborne epoxy resin emulsion and the waterborne epoxy resin curing agent (409) were compounded according to the ratio of epoxy equivalent to active hydrogen equivalent of 1:1, and 0.1 parts of leveling agent, 0.05 parts of defoaming agent and 0.6 parts of wetting agent were added and stirred evenly. The mixture was stirred at a low speed for 30 minutes, and then filtered, discharged and packaged to prepare a waterborne epoxy resin varnish. After curing and forming a film on a mild steel plate (about 60 microns), the edge was sealed and dried in a ventilated place at room temperature for 7 days; after being completely dried for 7 days, the anti-corrosion performance was tested. The water resistance of the paint film was tested according to the national standard GB / T 1733-1993.

[0025] Example 2

[0026] Lignin extraction method: Crush corn stalks into stalk powder with a crusher. Weigh 10g corn stalk powder and 10g ethylene glycol and place them in a hydrothermal reactor, heat to 190 °C for 7 hours. After the reaction is completed, cool to room temperature. Filter the product after the reaction under reduced pressure, wash the product with ethylene glycol 3 times, separate the stalk residue from the lignin solution by centrifugation, add a large amount of water to the lignin solution and stir, lignin precipitates, and freeze-dry the obtained lignin to obtain brown powder lignin.

[0027] 6 g of purified lignin, 1.5 g of sodium hydride, and 10 g of dimethyl sulfoxide were placed in a container and reacted at room temperature for 30 min. Then, 1.5 g of 1,3-propane sultone was added, the temperature was raised to 70 °C, and the reactor was evacuated and filled with nitrogen three times. The reaction was repeated for 14 h to obtain the product sodium lignin sulfonate solution. Sodium lignin sulfonate powder was prepared by vacuum distillation and freeze drying.

[0028] Add 4 g of polyethylene glycol monomethyl ether, 2 g of sodium hydride, and 11 g of dimethyl sulfoxide to the container, react at room temperature for 30 min, then add 9 g of sodium lignin sulfonate, and heat to 110 °C under magnetic stirring. Vacuum and fill the reactor with nitrogen three times, and react for 14 h. After the reaction is completed, dimethyl sulfoxide is removed by vacuum distillation to obtain sodium lignin sulfonate-polyethylene glycol monomethyl ether.

[0029] Weigh 17 g of sodium lignin sulfonate-polyethylene glycol monomethyl ether and 2 g of sodium hydride in a container, use 11 g of ethylene glycol propyl ether as a solvent, react at room temperature for 30 min, then add 10 g of bisphenol A epoxy resin E44, raise the temperature to 90 °C, react for 16 h, evacuate the reactor and fill it with nitrogen three times, cool it to room temperature and discharge it to obtain a light yellow transparent biomass-based epoxy emulsifier.

[0030] Add 1.5 g of lignin emulsifier and 12.5 g of epoxy resin E-44 into a three-necked flask, and install a mechanical stirring paddle, a constant pressure funnel, and a condenser into the three-necked flask. Under stirring conditions, heat to 80 °C and preheat for 2 h. After preheating, lower the temperature to 60 °C, add 11 g of distilled water to the constant pressure dropping funnel, and increase the speed to 3000 r / min. Distilled water is slowly added dropwise into the reaction system, and the viscosity of the epoxy resin increases first and then decreases, that is, the phase inversion process. When all the deionized water is added dropwise, continue to slowly stir and keep warm for 1 h to obtain a milky water-based epoxy resin emulsion with a solid content of 55%.

[0031] The waterborne epoxy resin emulsion and the waterborne epoxy resin curing agent (409) were compounded according to the ratio of epoxy equivalent to active hydrogen equivalent of 1:1, and 0.1 parts of leveling agent, 0.05 parts of defoaming agent and 0.6 parts of wetting agent were added and stirred evenly. The mixture was stirred at a low speed for 30 minutes, and then filtered, discharged and packaged to prepare a waterborne epoxy resin varnish. After curing and forming a film on a mild steel plate (about 60 microns), the edge was sealed and dried in a ventilated place at room temperature for 7 days; after being completely dried for 7 days, the anti-corrosion performance was tested. The water resistance of the paint film was tested according to the national standard GB / T 1733-1993.

[0032] Example 3

[0033] Lignin extraction method: Crush corn stalks into stalk powder with a crusher. Weigh 5g corn stalk powder and 6g ethylene glycol and place them in a hydrothermal reactor. Heat to 200℃ for 8 hours. Cool to room temperature after the reaction. Filter the product after the reaction under reduced pressure, wash the product with ethylene glycol 3 times, separate the stalk residue from the lignin solution by centrifugation, add a large amount of water to the lignin solution and stir, precipitate the lignin, freeze-dry the obtained lignin, and obtain brown powder lignin.

[0034] 7 g of purified lignin, 2 g of sodium hydride, and 12 g of dimethyl sulfoxide were placed in a container and reacted at room temperature for 30 min. Then, 2 g of 1,3-propane sultone was added, the temperature was raised to 80 °C, and the reactor was evacuated and filled with nitrogen three times. The reaction was repeated for 16 h to obtain the product sodium lignin sulfonate solution. Sodium lignin sulfonate powder was prepared by vacuum distillation and freeze drying.

[0035] Add 5 g of polyethylene glycol monomethyl ether, 3 g of sodium hydride, and 12 g of dimethyl sulfoxide to the container, react at room temperature for 30 min, then add 10 g of sodium lignin sulfonate, and heat to 120 °C under magnetic stirring. Vacuum and fill the reactor with nitrogen three times, and react for 16 h. After the reaction is completed, dimethyl sulfoxide is removed by vacuum distillation to obtain sodium lignin sulfonate-polyethylene glycol monomethyl ether.

[0036] Weigh 18 g of sodium lignin sulfonate-polyethylene glycol monomethyl ether and 3 g of sodium hydride in a container, use 12 g of ethylene glycol propyl ether as a solvent, react at room temperature for 30 min, then add 11 g of bisphenol A epoxy resin E20, raise the temperature to 100 °C, react for 20 h, evacuate the reactor and fill it with nitrogen three times, cool it to room temperature and discharge it to obtain a light yellow transparent biomass-based epoxy emulsifier.

[0037] Add 1.5 g of lignin emulsifier and 12.5 g of epoxy resin E-44 into a three-necked flask, and install a mechanical stirring paddle, a constant pressure funnel, and a condenser into the three-necked flask. Under stirring conditions, heat to 80 °C and preheat for 2 h. After preheating, lower the temperature to 60 °C, add 11 g of distilled water to the constant pressure dropping funnel, and increase the speed to 3000 r / min. Distilled water is slowly added dropwise into the reaction system, and the viscosity of the epoxy resin increases first and then decreases, that is, the phase inversion process. When all the deionized water is added dropwise, continue to slowly stir and keep warm for 1 h to obtain a milky water-based epoxy resin emulsion with a solid content of 55%.

[0038] The waterborne epoxy resin emulsion and the waterborne epoxy resin curing agent (409) were compounded according to the ratio of epoxy equivalent to active hydrogen equivalent of 1:1, and 0.1 parts of leveling agent, 0.05 parts of defoaming agent and 0.6 parts of wetting agent were added and stirred evenly. The mixture was stirred at a low speed for 30 minutes, and then filtered, discharged and packaged to prepare a waterborne epoxy resin varnish. After curing and forming a film on a mild steel plate (about 60 microns), the edge was sealed and dried in a ventilated place at room temperature for 7 days; after being completely dried for 7 days, the anti-corrosion performance was tested. The water resistance of the paint film was tested according to the national standard GB / T 1733-1993.

[0039] Table 1 Evaluation of emulsion performance in Examples 1 to 3

[0040] serial number 1 month 2 months 3 months 1 Unstratified Layering Layering 2 Unstratified Unstratified Layering 3 Unstratified Unstratified Unstratified

[0041] Table 2 Evaluation of mechanical properties of emulsions in Examples 1 to 3

[0042] serial number 3500 r / min×30 min 1 Layering 2 Layering 3 Unstratified

[0043] Table 3 Performance evaluation of waterborne epoxy resin coatings in Examples 1 to 3

[0044] serial number Rust Foaming Acceleration Line 1 10 0 10 2 10 0 10 3 10 0 10

[0045] Note: Rust is graded from 0 to 10, with 10 being the best.

[0046] The foaming is divided into 0-5 levels, with 0 being no foam and 5 being intensive foam.

[0047] The acceleration line is from 0 to 10 levels, with 10 being the best. BRIEF DESCRIPTION OF THE DRAWINGS

[0048] Figure 1 The anti-corrosion coating prepared by the emulsion in Examples 1-3 of the present invention was sprayed on a steel plate of the same size, and the water resistance test diagram was obtained. Figure 1It can be seen from Tables 1-3 that the waterborne epoxy resin coating prepared by the present invention is relatively stable. When applied on a steel plate, no large-scale rust occurs on the surface of the steel plate, and no bubbles appear on the surface of the steel plate. The above indicates that the prepared epoxy resin coating has broad application prospects in the field of corrosion protection.

Claims

1. A method for preparing a biomass-based emulsifier for waterborne epoxy anticorrosive coating resin, characterized in that The method comprises the following steps: (1) extracting lignin: crush corn stalks, wheat stalks or cotton stalks into stalk powder by a grinder, weigh 100 parts of corn stalks, wheat stalks or cotton stalk powder and 100-120 parts of ethylene glycol, place them in a hydrothermal reactor, heat them to 180-200°C for 6-8 hours, and cool them to room temperature after the reaction is completed; filter the product after the reaction under reduced pressure, wash the product with ethylene glycol for 3 times, separate the stalk residue from the lignin solution by centrifugation, add a large amount of water to the lignin solution and stir, precipitate the lignin, freeze-dry the obtained lignin, and obtain brown powder lignin; (2) place 10-12 parts of purified lignin, 1-3 parts of sodium hydride and 10-16 parts of dimethyl sulfoxide in a container, react at room temperature for 30 minutes, then add 2-6 parts of 1,3-propane sultone, and heat to 60-80°C. ℃, evacuate the reactor and fill it with nitrogen three times, react for 12-16 hours to obtain the product sodium lignin sulfonate solution, and then distill under reduced pressure and freeze-dry to prepare sodium lignin sulfonate powder; (3) add 3-5 parts of polyethylene glycol monomethyl ether, 1-3 parts of sodium hydride, and 10-12 parts of dimethyl sulfoxide to the container, react at room temperature for 30 minutes, then add 8-10 parts of sodium lignin sulfonate, stir and heat to 100-120 ℃, evacuate the reactor and fill it with nitrogen three times, react for 12-16 hours, and after the reaction is completed, dimethyl sulfoxide is removed by distillation under reduced pressure to obtain sodium lignin sulfonate-polyethylene glycol monomethyl ether; (4) Weigh 16-18 parts of sodium lignin sulfonate-polyethylene glycol monomethyl ether, 1-3 parts of sodium hydride, and 10-12 parts of any one selected from ethylene glycol propyl ether, ethylene glycol methyl ether, ethylene glycol ethyl ether, propylene glycol methyl ether, propylene glycol ethyl ether, and propylene glycol propyl ether, or a mixture of any two or more thereof as a solvent and place them in a container, react at room temperature for 30 min, then add 9-11 parts of bisphenol A epoxy resin, increase the temperature to 80-100 ° C, react for 16-20 h, evacuate the reactor and fill it with nitrogen three times, cool it to room temperature and discharge it to obtain a light yellow transparent biomass-based epoxy emulsifier.

2. The method for preparing a biomass-based emulsifier according to claim 1, characterized in that: The polyethylene glycol monomethyl ether is any one of polyethylene glycol monomethyl ether M750, polyethylene glycol monomethyl ether M2000, and polyethylene glycol monomethyl ether M5000, or a mixture of any two or more thereof.

3. The method for preparing a biomass-based emulsifier according to claim 1, characterized in that: The bisphenol A epoxy resin is any one of bisphenol A epoxy resin E20, bisphenol A epoxy resin E44, and bisphenol A epoxy resin E51, or a mixture of any two or more thereof.