A synthetic magnesium alloy cutting fluid based on modified corrosion inhibitor and preparation method thereof
By using modified corrosion inhibitors and calcium-magnesium soap dispersants and other components, protective coordination polymers are formed, which solves the problem of corruption and decomposition of magnesium alloy cutting fluid, and improves the anti-corrosion, lubrication and defoaming properties of magnesium alloy , extends the service life of magnesium alloy cutting fluid.
Patent Information
- Application Number
- CN202310195053.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-03
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2043-03-03
AI Technical Summary
The existing magnesium alloy cutting fluid is prone to corrosion and decomposition failure during processing, resulting in the reduction of processing accuracy of the adhesion substances on the surface of the magnesium alloy, and the active magnesium alloy is easily corroded. The existing corrosion inhibitor has a short life and cannot effectively protect the magnesium alloy.
Modified corrosion inhibitors such as oleoyl sarcosine and benzotriazole, lauroyl sarcosine and benzotriazole, isononanoic acid oleoyl sarcosine and benzotriazole, combined with calcium-magnesium soap dispersant and rust-proof agent and lubricants to form protective coordination polymers to improve the corrosion and lubricating properties of the surface of magnesium alloys.
It extends the service life of magnesium alloy cutting fluid, improves the anti-corrosion, lubrication and defoaming properties of magnesium alloy, reduces the corrosion of magnesium alloy, and ensures the accuracy and efficiency of magnesium alloy processing.
Smart Images

Figure BDA0004106813740000091 
Figure BDA0004106813740000101
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of metal processing cutting fluids, and in particular to a synthetic magnesium alloy cutting fluid based on a modified corrosion inhibitor and a preparation method thereof. Background Art
[0002] Magnesium alloys are known as the green metal structural materials of the 21st century for their light weight, high specific strength, good thermal conductivity, excellent shock absorption and electromagnetic shielding, good recyclability and machining performance, high dimensional stability, strong buffering capacity for vibration and noise, low sensitivity to intergranular corrosion and stress corrosion cracking (SCC), and renewable and low pollution to the environment. They are widely used in automobiles, motorcycles, machinery, aviation, navigation, national defense, 3C products, hand tools and other fields.
[0003] At present, most of the existing magnesium alloy cutting fluids in China use phosphate esters or organosiloxane modified types as the main magnesium alloy corrosion inhibitors to prevent magnesium alloy corrosion and discoloration. Phosphate ester slow-release agents are prone to breeding bacteria, causing the cutting fluid to rot and deteriorate; the other type of organosiloxane modified magnesium alloy corrosion inhibitors have poor compatibility with phosphate ester formulas, are prone to decomposition and failure, and are prone to adhere to the surface of magnesium alloy workpieces, reducing the subsequent magnesium alloy anodizing efficiency and failing to provide effective protection for long-term processing of magnesium alloys. On the other hand, magnesium alloys are prone to produce Mg during processing. 2+ , resulting in Mg in the cutting fluid 2+ The sharp rise in concentration, Mg 2+ It forms magnesium soap with anionic emulsifiers in cutting fluid, such as fatty acids, which consumes a lot of emulsifiers, causing the cutting fluid to demulsify and stratify. Moreover, these metal magnesium soaps easily adhere to the surface of the machine, effectively reducing the processing accuracy of the product. In addition, magnesium alloys are very active, so it is urgent to find new magnesium alloy corrosion inhibitors and develop magnesium alloy cutting fluids with longer life and more stable corrosion inhibition effects. Summary of the invention
[0004] The purpose of the present invention is to overcome the shortcomings of the prior art and provide a synthetic magnesium alloy cutting fluid based on a modified corrosion inhibitor and a preparation method thereof. The synthetic magnesium alloy cutting fluid of the present invention has excellent magnesium sustained release performance, hydrogen release inhibition performance, lubrication performance, defoaming performance and calcium-magnesium soap dispersion performance.
[0005] To achieve the above purpose, the technical solution adopted by the present invention is: to provide a synthetic magnesium alloy cutting fluid based on a modified corrosion inhibitor, comprising the following components in parts by weight: 10 to 20 parts of an alkali reserve agent, 1 to 3 parts of a magnesium alloy corrosion inhibitor, 5 to 10 parts of a lubricant, 3 to 6 parts of a calcium magnesium soap dispersant, 3 to 5 parts of a coupling agent, 0.5 to 2 parts of an air release agent, 5 to 10 parts of a rust inhibitor, 3 to 5 parts of a bactericide and 30 to 50 parts of deionized water;
[0006] The magnesium alloy corrosion inhibitor is at least one of a derivative of oleoylsarcosine and benzotriazole, a derivative of lauroylsarcosine and benzotriazole, and a derivative of isononanoylsarcosine and benzotriazole.
[0007] Specifically, the preparation method of the derivative modified by oleoylsarcosine and benzotriazole is as follows: N-oleoylsarcosine and benzotriazole are mixed, and stirred for reaction at a temperature of 60-70° C. for 60-120 minutes to obtain the derivative; the mass ratio of N-oleoylsarcosine to benzotriazole is 1.5-2.5:1.
[0008] Specifically, the preparation method of the derivative modified by lauroyl sarcosine and benzotriazole is as follows: lauroyl sarcosine and benzotriazole are mixed, and stirred for reaction at a temperature of 60-70° C. for 60-120 min to obtain the derivative; the mass ratio of lauroyl sarcosine to benzotriazole is 1.5-2.5:1.
[0009] Specifically, the preparation method of the derivative modified by isononanoic acid oleoyl sarcosine and benzotriazole is as follows:
[0010] First, N-oleoylsarcosine-octadecylamine salt and isononanoic acid are mixed, and stirred at a temperature of 40-50° C. for 60-120 minutes to obtain isononanoic acid oleoylsarcosine; wherein the mass ratio of N-oleoylsarcosine-octadecylamine salt to isononanoic acid is 0.9-1.1:1;
[0011] Then the obtained isononanoic acid oleoyl sarcosine and benzotriazole are mixed, and stirred for reaction at a temperature of 60-70° C. for 60-120 min to obtain the product; the mass ratio of the isononanoic acid oleoyl sarcosine to benzotriazole is 1.5-2.5:1.
[0012] In the components of the synthetic magnesium alloy cutting fluid of the present invention, at least one of the derivatives modified by oleoylsarcosine and benzotriazole, the derivatives modified by lauroylsarcosine and benzotriazole, and the derivatives modified by isononanoylsarcosine and benzotriazole is added as a magnesium alloy corrosion inhibitor. At a higher pH value, the magnesium alloy corrosion inhibitor of the present invention forms a protective coordination polymer with metal ions in the magnesium alloy. At a lower pH value, the magnesium alloy corrosion inhibitor of the present invention is chemically adsorbed on the surface of the magnesium alloy. Moreover, the magnesium alloy corrosion inhibitor of the present invention forms a surface film with greater hydrophobicity, fewer defects, and greater durability on the surface of the magnesium alloy, thereby effectively separating the corrosive medium from the surface of the magnesium alloy and reducing the corrosion of the magnesium alloy. The magnesium alloy corrosion inhibitor of the present invention is adapted to a wider pH range and has a more lasting protective effect on magnesium. On the one hand, the magnesium alloy corrosion inhibitor of the present invention works together with the rust inhibitor to improve the anti-corrosion performance of the product. By selecting a specific magnesium alloy corrosion inhibitor and compounding with other components, the synthetic magnesium alloy cutting fluid has an excellent non-ferrous metal sustained-release effect. On the other hand, the magnesium alloy corrosion inhibitor of the present invention works together with the calcium-magnesium soap dispersant to improve the defoaming performance of the product.
[0013] As a preferred embodiment of the synthetic magnesium alloy cutting fluid of the present invention, the calcium magnesium soap dispersant is at least one of hydroxyhexylidene diphosphonic acid, ethylenediamine tetramethylene phosphonic acid, and polyaspartic acid.
[0014] In the components of the synthetic magnesium alloy cutting fluid of the present invention, the mutual matching of the calcium-magnesium soap dispersant and the amine in the alkali reserve agent enables the synthetic fluid to have high calcium-magnesium soap dispersibility and prolong the service life of the working fluid.
[0015] As a preferred embodiment of the synthetic magnesium alloy cutting fluid of the present invention, the coupling agent is at least one of polyisobutylene succinic anhydride, polyisobutylene succinic anhydride potassium salt, polyisobutylene succinic anhydride sodium salt, and polyisobutylene succinic anhydride ammonium salt. The coupling agent of the present invention has a good lubricating effect. After adding the coupling agent, the dispersion stability of the cutting fluid can be improved, and the defoaming ability of the product can be improved. The molecular weight of the coupling agent is one of the main factors affecting the stability of the product. If the molecular weight of the coupling agent is small, adding the coupling agent will cause the stability of the product to deteriorate. If the molecular weight of the coupling agent is too large, adding the coupling agent will reduce the defoaming ability of the product. Preferably, the average molecular weight of the coupling agent is 1000.
[0016] The preparation method of the polyisobutylene succinic anhydride salt of the present invention is as follows: polyisobutylene succinic anhydride and component A are stirred and reacted at room temperature for 60-120 minutes to obtain the product; wherein component A is one of 10% KOH aqueous solution, 0% NaOH aqueous solution and organic amine, and the organic amine is one of methyldiethanolamine, butyl-monoethanolamine, butyl-diethanolamine and octyl-diethanolamine; and the mass ratio of polyisobutylene succinic anhydride to component A is 1.5-2.5:1.
[0017] As a preferred embodiment of the synthetic magnesium alloy cutting fluid of the present invention, the rust inhibitor is at least one of C22-tribasic acid, 21-carbon dibasic acid, isodecanoic acid, and N-acylamino acid.
[0018] The present invention selects a specific rust inhibitor to optimize the emulsification type and rust resistance of the product of the present invention. Adding the rust inhibitor to the cutting fluid of the present invention can effectively improve the dispersibility and rust resistance of the cutting fluid, so that the cutting fluid forms a microemulsion with extremely small particles after being diluted with a large amount of water, and works together with the calcium-magnesium soap dispersant to improve the calcium-magnesium dispersibility of the product.
[0019] As a preferred embodiment of the synthetic magnesium alloy cutting fluid of the present invention, the alkali reserve agent is at least one of methyldiethanolamine, butyl-monoethanolamine, butyl-diethanolamine, and octyl-diethanolamine.
[0020] As a preferred embodiment of the synthetic magnesium alloy cutting fluid of the present invention, the lubricant is at least one of hydrogenated rapeseed oil polyoxyethylene ether, hydrogenated palm oil polyoxyethylene ether, hydrogenated castor oil polyoxyethylene ether, and hydrogenated soybean oil polyoxyethylene ether.
[0021] The lubricant has good oxidation stability, high hydrolysis stability, is renewable and degradable, and has good lubrication properties, and can improve the lubrication properties of synthetic magnesium alloy cutting fluids.
[0022] Those skilled in the art can purchase commercial products as the lubricant of the present invention, or prepare the lubricant of the present invention according to conventional preparation methods in the art; for example, hydrogenated vegetable oil, boron trifluoride ethyl ether and ethylene oxide are added to a reactor, and reacted at 100-120° C. to obtain the lubricant; wherein the hydrogenated vegetable oil is one of hydrogenated castor oil, hydrogenated rapeseed oil, hydrogenated soybean oil, and hydrogenated palm oil, and the mass ratio of boron trifluoride ethyl ether is 0.8-1.3% of the mass of the hydrogenated vegetable oil.
[0023] As a preferred embodiment of the synthetic magnesium alloy cutting fluid of the present invention, the air release agent is polyetheramine.
[0024] As a preferred embodiment of the synthetic magnesium alloy cutting fluid of the present invention, the weight average molecular weight of the polyetheramine is 1500-2500.
[0025] The addition of polyetheramine can significantly improve the defoaming performance of cutting fluid, effectively prevent the generation of foam during high-speed grinding, thereby inhibiting the cutting fluid airflow barrier and preventing workpiece burns. Preferably, the weight average molecular weight of the polyetheramine is 1500-2500, and the defoaming performance of the polyetheramine in this molecular weight range is better; more preferably, the weight average molecular weight of the polyetheramine is 2000, and its primary amine group is connected to the second carbon atom of the end group of the aliphatic polyether main chain.
[0026] As a preferred embodiment of the synthetic magnesium alloy cutting fluid of the present invention, the bactericide is 1,2-benzisothiazolin-3-one, n-butyl-1,2-benzisothiazolin-3-one, and iodopropynyl butylcarbamate.
[0027] On the other hand, the present invention provides a method for preparing a synthetic magnesium alloy cutting fluid, comprising the following steps: mixing and stirring an alkali reserve agent, a magnesium alloy corrosion inhibitor, a lubricant and a calcium-magnesium soap dispersant evenly, then adding deionized water, a coupling agent and a rust inhibitor and mixing and stirring and evenly dissolving them, and finally adding a bactericide and an air release agent, stirring for 1 to 1.5 hours to obtain a synthetic magnesium alloy cutting fluid.
[0028] Compared with the prior art, the present invention has the following beneficial effects:
[0029] (1) At least one of the derivatives of oleoylsarcosine and benzotriazole modified, the derivatives of lauroylsarcosine and benzotriazole modified, and the derivatives of isononanoylsarcosine and benzotriazole modified is added to the components of the synthetic magnesium alloy cutting fluid of the present invention as a magnesium alloy corrosion inhibitor. On the one hand, the magnesium alloy corrosion inhibitor of the present invention works together with the rust inhibitor to improve the corrosion resistance of the product. A specific magnesium alloy corrosion inhibitor is selected and compounded with other components to make the synthetic magnesium alloy cutting fluid have an excellent non-ferrous metal sustained-release effect. On the other hand, the magnesium alloy corrosion inhibitor of the present invention works together with the calcium-magnesium soap dispersant to improve the defoaming performance of the product. The mutual matching of the calcium-magnesium soap dispersant and the amine in the alkali reserve agent makes the synthetic fluid have high calcium-magnesium soap dispersibility, thereby extending the service life of the working fluid.
[0030] (2) The present invention selects a specific rust inhibitor to optimize the emulsification type and rust resistance of the product of the present invention. Adding a rust inhibitor to the cutting fluid of the present invention can effectively improve the dispersibility and rust resistance of the cutting fluid, so that after the cutting fluid is diluted with a large amount of water, a microemulsion with extremely small particles is formed, which works together with the calcium-magnesium soap dispersant to improve the calcium-magnesium dispersibility of the product.
[0031] (3) The synthetic magnesium alloy cutting fluid of the present invention has excellent magnesium sustained-release performance, hydrogen release inhibition performance, lubrication performance, anti-foaming performance and calcium-magnesium soap dispersion performance, can meet the machining requirements of magnesium alloys, prevent discoloration of magnesium alloys, and effectively inhibit hydrogen release during magnesium alloy processing. DETAILED DESCRIPTION
[0032] In order to better illustrate the purpose, technical solutions and advantages of the present invention, the present invention will be further described below in conjunction with specific embodiments and comparative examples, the purpose of which is to understand the content of the present invention in detail, rather than to limit the present invention. All other embodiments obtained by those of ordinary skill in the art without making creative work premise belong to the protection scope of the present invention. The experimental reagents and instruments involved in the implementation of the present invention, unless otherwise specified, are all commonly used common reagents and instruments.
[0033] The raw materials used in the embodiments and comparative examples are described below, but are not limited to these materials:
[0034] The derivative modified by oleoylsarcosine and benzotriazole is homemade, and the preparation method is as follows: N-oleoylsarcosine and benzotriazole are mixed, and the mixture is stirred and reacted at a temperature of 65° C. for 90 minutes to obtain the derivative; wherein the mass ratio of N-oleoylsarcosine to benzotriazole is 2:1.
[0035] The derivative modified by lauroyl sarcosine and benzotriazole is homemade, and the preparation method is: mix lauroyl sarcosine and benzotriazole, and stir and react at a temperature of 65°C for 90 minutes to obtain the derivative; wherein the mass ratio of lauroyl sarcosine to benzotriazole is 2:1.
[0036] The derivative modified by isononanoic acid oleoyl sarcosine and benzotriazole is homemade, and the preparation method is as follows:
[0037] First, N-oleoylsarcosine-octadecylamine salt and isononanoic acid are mixed, and stirred for reaction at a temperature of 45° C. for 90 minutes to obtain isononanoic acid oleoylsarcosine; wherein the mass ratio of N-oleoylsarcosine-octadecylamine salt to isononanoic acid is 1:1;
[0038] Then the obtained isononanoic acid oleoyl sarcosine and benzotriazole are mixed, and stirred for reaction at a temperature of 65° C. for 90 minutes to obtain the product; wherein the mass ratio of isononanoic acid oleoyl sarcosine to benzotriazole is 2:1.
[0039] Polyetheramine D-2000 polyetheramine (D2000 polyamine ether).
[0040] Example 1
[0041] An embodiment of the synthetic magnesium alloy cutting fluid of the present invention, the synthetic magnesium alloy cutting fluid described in this embodiment is composed of the following components in parts by weight: 15 parts of methyldiethanolamine, 2 parts of oleoylsarcosine and benzotriazole modified derivatives, 10 parts of hydrogenated rapeseed oil polyoxyethylene ether, 5 parts of hydroxyhexylidene diphosphonic acid, 3 parts of polyisobutenyl succinic anhydride, 5 parts of C22-tribasic acid, 1 part of D2000 polyetheramine, 3 parts of 1,2-benzisothiazolin-3-one and 56 parts of deionized water; wherein the average molecular weight of the polyisobutenyl succinic anhydride is 1000.
[0042] The preparation method of the synthetic magnesium alloy cutting fluid described in this embodiment is as follows: first, methyldiethanolamine, acylsarcosine and benzotriazole-modified derivatives, hydrogenated rapeseed oil polyoxyethylene ether, and hydroxyhexylidene diphosphonic acid are added to a reactor, and after stirring evenly, deionized water, polyisobutenyl succinic anhydride with a molecular weight of 1000, and C22-tribasic acid are added, and stirring is performed until the solid is completely dissolved. Finally, D2000 polyetheramine and a bactericide are added, and the mixture is stirred at room temperature for 1 hour to obtain the synthetic magnesium alloy cutting fluid.
[0043] Example 2
[0044] An embodiment of the synthetic magnesium alloy cutting fluid of the present invention, the synthetic magnesium alloy cutting fluid described in this embodiment is composed of the following components in parts by weight: 15 parts of butyl-monoethanolamine, 2 parts of lauroyl sarcosine and benzotriazole-modified derivatives, 10 parts of hydrogenated palm oil polyoxyethylene ether, 3 parts of polyisobutylene succinic anhydride potassium salt, 5 parts of ethylenediaminetetramethylphosphonic acid, 5 parts of 21-carbon dibasic acid, 1 part of D2000 polyetheramine, 3 parts of 1,2-benzisothiazolin-3-one and 56 parts of deionized water; wherein the average molecular weight of polyisobutylene succinic anhydride potassium salt is 1000.
[0045] The specific preparation method of the synthetic magnesium alloy cutting fluid described in this embodiment is the same as that in Embodiment 1, the only difference being that the composition and weight proportion of each component of the cutting fluid are different.
[0046] Example 3
[0047] An embodiment of the synthetic magnesium alloy cutting fluid of the present invention, the synthetic magnesium alloy cutting fluid described in this embodiment is composed of the following components in parts by weight: 15 parts of butyl-diethanolamine, 2 parts of isononanoic acid oleoyl sarcosine and benzotriazole modified derivatives, 10 parts of hydrogenated castor oil polyoxyethylene ether, 3 parts of polyisobutylene succinic anhydride sodium salt, 5 parts of polyaspartic acid, 5 parts of isodecanic acid, 1 part of D2000 polyetheramine, 3 parts of 1,2-benzisothiazolin-3-one and 56 parts of deionized water; wherein the average molecular weight of polyisobutylene succinic anhydride potassium salt is 1000.
[0048] The specific preparation method of the synthetic magnesium alloy cutting fluid described in this embodiment is the same as that in Embodiment 1, the only difference being that the composition and weight proportion of each component of the cutting fluid are different.
[0049] Example 4
[0050] An embodiment of the synthetic magnesium alloy cutting fluid of the present invention, the synthetic magnesium alloy cutting fluid described in this embodiment is composed of the following components in parts by weight: 15 parts of octyl-diethanolamine, 2 parts of oleoyl sarcosine and benzotriazole modified derivatives, 10 parts of hydrogenated soybean oil polyoxyethylene ether, 3 parts of polyisobutylene succinic anhydride potassium salt, 5 parts of hydroxyhexylidene diphosphonic acid, 5 parts of monoacyl amino acid, 1 part of D2000 polyetheramine, 3 parts of 1,2-benzisothiazolin-3-one and 56 parts of deionized water; wherein the average molecular weight of polyisobutylene succinic anhydride potassium salt is 1000.
[0051] The specific preparation method of the synthetic magnesium alloy cutting fluid described in this embodiment is the same as that in Embodiment 1, the only difference being that the composition and weight proportion of each component of the cutting fluid are different.
[0052] Example 5
[0053] An embodiment of the synthetic magnesium alloy cutting fluid of the present invention, the synthetic magnesium alloy cutting fluid described in this embodiment is composed of the following components in parts by weight: 10 parts of methyldiethanolamine, 1 part of oleoylsarcosine and benzotriazole modified derivatives, 5 parts of hydrogenated rapeseed oil polyoxyethylene ether, 3 parts of hydroxyhexylidene diphosphonic acid, 4 parts of polyisobutenyl succinic anhydride, 8 parts of C22-tribasic acid, 0.5 parts of D2000 polyetheramine, 4 parts of 1,2-benzisothiazolin-3-one and 56 parts of deionized water; wherein the average molecular weight of the polyisobutenyl succinic anhydride is 1000.
[0054] The specific preparation method of the synthetic magnesium alloy cutting fluid described in this embodiment is the same as that in Embodiment 1, the only difference being that the composition and weight proportion of each component of the cutting fluid are different.
[0055] Example 6
[0056] An embodiment of the synthetic magnesium alloy cutting fluid of the present invention, the synthetic magnesium alloy cutting fluid described in this embodiment is composed of the following components in parts by weight: 20 parts of methyldiethanolamine, 3 parts of oleoylsarcosine and benzotriazole modified derivatives, 8 parts of hydrogenated rapeseed oil polyoxyethylene ether, 6 parts of hydroxyhexylidene diphosphonic acid, 5 parts of polyisobutenyl succinic anhydride, 10 parts of C22-tribasic acid, 2 parts of D2000 polyetheramine, 5 parts of 1,2-benzisothiazolin-3-one and 56 parts of deionized water; wherein the average molecular weight of the polyisobutenyl succinic anhydride is 1000.
[0057] The specific preparation method of the synthetic magnesium alloy cutting fluid described in this embodiment is the same as that in Embodiment 1, the only difference being that the composition and weight proportion of each component of the cutting fluid are different.
[0058] Comparative Example 1
[0059] A comparative example of the synthetic magnesium alloy cutting fluid of the present invention. The only difference between this comparative example and Example 1 is that the magnesium alloy corrosion inhibitor in the synthetic magnesium alloy cutting fluid of this comparative example is benzotriazole.
[0060] Comparative Example 2
[0061] A comparative example of the synthetic magnesium alloy cutting fluid of the present invention. The only difference between this comparative example and Example 1 is that the synthetic magnesium alloy cutting fluid described in this comparative example does not contain derivatives modified by oleoylsarcosine and benzotriazole.
[0062] Comparative Example 3
[0063] A comparative example of the synthetic magnesium alloy cutting fluid of the present invention. The only difference between this comparative example and Example 1 is that the synthetic magnesium alloy cutting fluid described in this comparative example does not contain hydroxyhexylidene diphosphonic acid.
[0064] Comparative Example 4
[0065] A comparative example of the synthetic magnesium alloy cutting fluid of the present invention. The only difference between this comparative example and Example 1 is that the synthetic magnesium alloy cutting fluid described in this comparative example does not contain oleoylsarcosine and benzotriazole-modified derivatives and hydroxyhexylidene diphosphonic acid.
[0066] Comparative Example 5
[0067] A comparative example of the synthetic magnesium alloy cutting fluid of the present invention. The only difference between this comparative example and Example 1 is that the synthetic magnesium alloy cutting fluid described in this comparative example does not contain C22-tribasic acid and oleoylsarcosine and benzotriazole-modified derivatives.
[0068] Comparative Example 6
[0069] A comparative example of the synthetic magnesium alloy cutting fluid of the present invention. The only difference between this comparative example and Example 1 is that the synthetic magnesium alloy cutting fluid described in this comparative example does not contain C22-tribasic acid and D2000 polyether amine.
[0070] Effect Example 1
[0071] The synthetic magnesium alloy cutting fluids prepared in Examples 1-6 and Comparative Examples 1-7 were diluted with deionized water to a dilution with a mass fraction of 5%, and then the performance was tested.
[0072] The test method for the dispersibility of calcium magnesium soap is as follows: according to the preparation method of standard hard water, different levels of hard water are prepared with anhydrous calcium chloride and anhydrous magnesium sulfate. The levels of hard water are 300ppm, 500ppm, 800ppm, 1000ppm, 1200ppm, 1500ppm, 3000ppm, 5000ppm, 8000ppm and 10000ppm respectively;
[0073] 5% hard water of different grades was added to the deionized water in each embodiment and comparative example to prepare a cutting fluid; the obtained cutting fluid was then diluted and the state of the diluted fluid was observed. No more than 1% soap could be precipitated within 24 hours; the hard water resistance grade of the cutting fluid was determined through step-by-step tests.
[0074] Other performance test methods and results are shown in Table 1 below.
[0075] Table 1
[0076]
[0077]
[0078] It can be seen from Table 1 that the synthetic magnesium alloy cutting fluid prepared in the embodiment of the present invention has excellent magnesium sustained release performance, hydrogen release inhibition performance, lubrication performance, defoaming performance and calcium-magnesium soap dispersibility.
[0079] Finally, it should be noted that the above embodiments are used to illustrate the technical solution of the present invention rather than to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.
Claims
1. A synthetic magnesium alloy cutting fluid based on a modified corrosion inhibitor, characterized in that: The invention comprises the following components in parts by weight: 10-20 parts of alkali reserve agent, 1-3 parts of magnesium alloy corrosion inhibitor, 5-10 parts of lubricant, 3-6 parts of calcium magnesium soap dispersant, 3-5 parts of coupling agent, 0.5-2 parts of air release agent, 5-10 parts of rust inhibitor, 3-5 parts of bactericide and 30-50 parts of deionized water; The magnesium alloy corrosion inhibitor is at least one of a derivative of oleoylsarcosine and benzotriazole, a derivative of lauroylsarcosine and benzotriazole, and a derivative of isononanoic acid and oleoylsarcosine and benzotriazole; The calcium magnesium soap dispersant is at least one of hydroxyhexylidene diphosphonic acid, ethylenediamine tetramethylene phosphonic acid, and polyaspartic acid; The coupling agent is at least one of polyisobutylene succinic anhydride, polyisobutylene succinic anhydride potassium salt, polyisobutylene succinic anhydride sodium salt, and polyisobutylene succinic anhydride ammonium salt.
2. The synthetic magnesium alloy cutting fluid according to claim 1, characterized in that: The rust inhibitor is at least one of C22-tribasic acid, 21-carbon dibasic acid, isodecanoic acid, and monobasic acylamino acid.
3. The synthetic magnesium alloy cutting fluid according to claim 1, characterized in that: The alkali reserve agent is at least one of methyldiethanolamine, butyl-monoethanolamine, butyl-diethanolamine, and octyl-diethanolamine.
4. The synthetic magnesium alloy cutting fluid according to claim 1, characterized in that: The lubricant is at least one of hydrogenated rapeseed oil polyoxyethylene ether, hydrogenated palm oil polyoxyethylene ether, hydrogenated castor oil polyoxyethylene ether, and hydrogenated soybean oil polyoxyethylene ether.
5. The synthetic magnesium alloy cutting fluid according to claim 1, characterized in that: The air release agent is polyetheramine.
6. The synthetic magnesium alloy cutting fluid according to claim 5, characterized in that: The weight average molecular weight of the polyetheramine is 1500-2500.
7. The synthetic magnesium alloy cutting fluid according to claim 1, characterized in that: The bactericide is 1,2-benzisothiazolin-3-one, n-butyl-1, 2-benzisothiazolin-3-one, and iodopropynyl butyl carbamate.
8. The method for preparing a synthetic magnesium alloy cutting fluid according to any one of claims 1 to 7, characterized in that: The method comprises the following steps: mixing and stirring an alkali reserve agent, a magnesium alloy corrosion inhibitor, a lubricant and a calcium-magnesium soap dispersant evenly, then adding deionized water, a coupling agent and a rust inhibitor and mixing and stirring and dissolving evenly, and finally adding a bactericide and an air release agent and stirring for 1 to 1.5 hours to obtain a synthetic magnesium alloy cutting fluid.