A high-stability cationic lignin rosin sizing agent, preparation method and application
By classifying lignin and reacting with substances such as epichlorohydrin, triethylamine and polyacrylamide, a highly stable cationic lignin rosin sizing agent is prepared, which solves the problem of poor stability of rosin sizing agents and improves the quality of paper or cardboard It has excellent hydrophobic and strength properties and is suitable for the production of liquid packaging cardboard.
Patent Information
- Application Number
- CN202310174028.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-02-28
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2043-02-28
AI Technical Summary
The poor stability of existing rosin sizing agents leads to a decrease in the physical strength and poor hydrophobic properties of paper or cardboard, affecting its application in production.
By classifying lignin powder and reacting it with epichlorohydrin and triethylamine in a strong alkaline solution, and then dispersing it with cationic polyacrylamide and nonionic polyacrylamide in deionized water, and homogenizing it under high pressure, a highly stable lignin powder was prepared. Sexual cationic lignin rosin sizing agent.
It improves the stability and hydrophobic properties of rosin sizing agent, enhances the physical strength of paper or cardboard, and extends the storage time. It is suitable for the preparation of liquid packaging cardboard.
Smart Images

Figure CN116377757B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of rosin sizing agent processing, in particular to a high-stability cationic lignin rosin sizing agent, a preparation method and application thereof. Background Art
[0002] Sizing treatment is the most common method to improve the hydrophobicity of paper or paperboard. Rosin is the most important internal sizing agent in the production process of paper or paperboard because it has low cost, wide source of raw materials, simple and easy to control sizing process, and high compatibility with pulp fibers and other sizing agents. The functional groups of rosin are mainly conjugated unsaturated double bonds and carboxyl groups. During the rosin sizing process, the polar carboxyl groups react with the hydrophilic paper surface to orient the non-polar unsaturated double bonds to form a stable hydrophobic surface with reduced free energy. However, due to the barrier effect of rosin between pulp fibers and the low retention rate of rosin, the presence of rosin particles will cause the physical strength of paper or paperboard to decrease. In addition, the poor stability of rosin sizing agents will cause the rosin sizing agents to demulsify during storage, reduce their sizing effect, and thus affect their application in actual production. Therefore, improving the stability of the sizing agent while improving the hydrophobicity and strength properties of paper or paperboard is a problem that needs to be solved in the current sizing agent field.
[0003] Patent application No. 201710694208.1 discloses an alkaline sizing agent in a cationic rosin emulsion, which can improve the glossiness of paper, and has good surface strength after sizing, and significantly improves dry and wet strength. However, its preparation process is complicated, and the performance of the emulsion sizing agent is not stable enough, and the storage time is short.
[0004] Therefore, it can be seen that the rosin sizing agent in the prior art cannot fully meet the needs of users, so a new rosin sizing agent is urgently needed. Summary of the invention
[0005] The purpose of the present invention is to overcome the deficiencies in the prior art and provide a high-stability cationic lignin rosin sizing agent, a preparation method and an application thereof.
[0006] The technical solution adopted by the present invention to solve its technical problem is:
[0007] A method for preparing a high-stability cationic lignin rosin sizing agent, the method comprising the following steps:
[0008] (1) dissolving lignin powder in ethanol aqueous solutions of different concentrations respectively, stirring, standing and filtering, and drying the filter residue and the filtrate respectively to obtain graded lignin with different molecular weights; wherein the graded lignin is lignin with the following three molecular weight distribution ranges: lignin with a molecular weight distribution range greater than 5000 g / mol; lignin with a molecular weight distribution range of 3000 to 5000 g / mol; and lignin with a molecular weight distribution range less than 3000 g / mol;
[0009] (2) mixing fractionated lignin with different molecular weights with epichlorohydrin in a strong alkaline solution, stirring and filtering to obtain a solid product; mixing the solid product with triethylamine in a dilute alkaline solution, and adjusting the pH value of the solution to acidity with hydrochloric acid after the reaction is completed; filtering and washing the obtained solid with deionized water, repeating this process until the solid is neutral, and then drying the product under conditions;
[0010] (3) heating and melting solid rosin into uniform rosin liquid; dispersing the product in step (2) with cationic polyacrylamide (CPAM) and nonionic polyacrylamide (NPAM) in deionized water, and stirring to obtain a uniform emulsifier; mixing the emulsifier and the rosin liquid and homogenizing under high pressure to obtain a highly stable cationic lignin rosin sizing agent.
[0011] Furthermore, the mass concentration of the ethanol aqueous solution in step (1) is 95% and 70%;
[0012] Alternatively, the stirring time in step (1) is 10 to 60 minutes.
[0013] Furthermore, in step (2), the mass ratio of lignin, epichlorohydrin, and triethylamine is 1:1-5:1-5;
[0014] Alternatively, the strong alkaline solution in step (2) is 60 ml of 3-7 mol / L sodium hydroxide solution;
[0015] Alternatively, the stirring conditions in step (2) are: 50-80° C., 500-1000 rpm, 2-5 h.
[0016] Furthermore, in step (2), the dilute alkaline solution is 60 ml of 0.1-1 mol / L sodium hydroxide solution;
[0017] Alternatively, the drying conditions in step (2) are: 30-80° C., 8-20 h.
[0018] Furthermore, in step (3), the mass ratio of the product, cationic polyacrylamide, nonionic polyacrylamide, rosin liquid, and deionized water is 0.5-5:0.5-5:0.5-5:50-100:50-100;
[0019] Alternatively, the stirring conditions in step (3) are: 50-100° C., 500-2000 rpm;
[0020] Alternatively, the conditions for high pressure homogenization in step (3) are: 20-60 MPa, 5-30 min.
[0021] The high-stability cationic lignin rosin sizing agent is prepared by the method as described above.
[0022] The application of the high stability cationic lignin rosin sizing agent as described above in the preparation of liquid packaging paperboard.
[0023] The method for making liquid packaging paperboard base paper using the high-stability cationic lignin rosin sizing agent as described above comprises the following steps:
[0024] Highly stable cationic lignin rosin sizing agent emulsion is added into pulp to produce liquid packaging paperboard base paper.
[0025] Furthermore, in step (4), the amount of the high-stability cationic lignin rosin sizing agent added is 10 to 30 kg / ton of pulp.
[0026] Furthermore, in step (4), the basis weight of the liquid packaging paperboard base paper is 80 to 200 g / m 2 .
[0027] The advantages and positive effects achieved by the present invention are:
[0028] 1. The method of the present invention pioneered the exploration of fractionated lignin to improve the stability of rosin sizing agents, and applied it to the field of liquid packaging paperboard to improve the hydrophobicity and strength properties of paperboard. The method of the present invention solves the problem of poor stability of existing rosin sizing agents. At the same time, the rosin sizing agent obtained by the method of the present invention can improve the stability of the sizing agent and ensure the sizing effect.
[0029] 2. The rosin sizing agent obtained by the method of the present invention can improve the hydrophobicity of paperboard.
[0030] 3. The rosin sizing agent obtained by the method of the present invention can improve the strength performance of paperboard.
[0031] 4. The present invention provides a stable and sustainable approach for the utilization of lignin. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] Figure 1 This is a comparison chart of the molecular weight and polydispersity index (PDI) of different fractions of lignin in Examples 1-3 of the present invention;
[0033] Figure 2 It is a two-dimensional NMR comparison diagram of different fractions of lignin in Examples 1-3 of the present invention;
[0034] Figure 3 It is a comparison diagram of the particle size and polydispersity index (PDI) of cationic lignin rosin sizing agents of different sizes in Examples 1-3 of the present invention; wherein, Figure a is a comparison diagram of the particle size of the sizing agent, and Figure b is a polydispersity index (PDI) of the sizing agent particles;
[0035] Figure 4 This is a comparison chart of the Zeta potential of cationic lignin rosin sizing agents of different sizes in Examples 1-3 of the present invention;
[0036] Figure 5 It is a comparison chart of the Cobb values of Examples 1-3 and Comparative Examples 1-4 in the present invention; wherein, Figure a is a comparison chart of the Cobb values of Examples 1-3 and Comparative Examples 1-4, and Figure b is a comparison chart of the Cobb values of Examples 1-3 and Comparative Examples 2-4;
[0037] Figure 6 It is a comparison diagram of the contact angles of Examples 1-3 and Comparative Examples 1-4 in the present invention;
[0038] Figure 7 It is a comparison chart of the tensile index of Examples 1-3 and Comparative Examples 1-4 in the present invention. DETAILED DESCRIPTION
[0039] The present invention will be further described below in conjunction with the embodiments. The following embodiments are descriptive rather than restrictive, and the protection scope of the present invention cannot be limited by the following embodiments.
[0040] The various experimental operations involved in the specific embodiments are all routine techniques in the art. For parts not specially annotated in this document, ordinary technicians in the art can implement them by referring to various commonly used reference books, scientific and technological literature or related instructions, manuals, etc. before the filing date of this invention.
[0041] A method for preparing a high-stability cationic lignin rosin sizing agent, the method comprising the following steps:
[0042] (1) dissolving lignin powder in ethanol aqueous solutions of different concentrations respectively, stirring, standing and filtering, and drying the filter residue and the filtrate respectively to obtain graded lignin with different molecular weights; wherein the graded lignin is lignin with the following three molecular weight distribution ranges: lignin with a molecular weight distribution range greater than 5000 g / mol; lignin with a molecular weight distribution range of 3000 to 5000 g / mol; and lignin with a molecular weight distribution range less than 3000 g / mol;
[0043] (2) mixing fractionated lignin with different molecular weights with epichlorohydrin in a strong alkaline solution, stirring and filtering to obtain a solid product; mixing the solid product with triethylamine in a dilute alkaline solution, and adjusting the pH value of the solution to acidity with hydrochloric acid after the reaction is completed; filtering and washing the obtained solid with deionized water, repeating this process until the solid is neutral, and then drying the product under conditions;
[0044] (3) heating and melting solid rosin into uniform rosin liquid; dispersing the product in step (2) with cationic polyacrylamide (CPAM) and nonionic polyacrylamide (NPAM) in deionized water, and stirring to obtain a uniform emulsifier; mixing the emulsifier and the rosin liquid and homogenizing under high pressure to obtain a highly stable cationic lignin rosin sizing agent.
[0045] Preferably, the mass concentration of the ethanol aqueous solution in step (1) is 95% and 70%;
[0046] Alternatively, the stirring time in step (1) is 10 to 60 minutes.
[0047] Preferably, in step (2), the mass ratio of lignin, epichlorohydrin, and triethylamine is 1:1-5:1-5;
[0048] Alternatively, the strong alkaline solution in step (2) is 60 ml of 3-7 mol / L sodium hydroxide solution;
[0049] Alternatively, the stirring conditions in step (2) are: 50-80° C., 500-1000 rpm, 2-5 h.
[0050] Preferably, the dilute alkaline solution in step (2) is 60 ml of 0.1-1 mol / L sodium hydroxide solution;
[0051] Alternatively, the drying conditions in step (2) are: 30-80° C., 8-20 h.
[0052] Furthermore, in step (3), the mass ratio of the product, cationic polyacrylamide, nonionic polyacrylamide, rosin liquid, and deionized water is 0.5-5:0.5-5:0.5-5:50-100:50-100;
[0053] Alternatively, the stirring conditions in step (3) are: 50-100° C., 500-2000 rpm;
[0054] Alternatively, the conditions for high pressure homogenization in step (3) are: 20-60 MPa, 5-30 min.
[0055] The high-stability cationic lignin rosin sizing agent is prepared by the method as described above.
[0056] The application of the high stability cationic lignin rosin sizing agent as described above in the preparation of liquid packaging paperboard.
[0057] The method for making liquid packaging paperboard base paper using the high-stability cationic lignin rosin sizing agent as described above comprises the following steps:
[0058] Highly stable cationic lignin rosin sizing agent emulsion is added into pulp to produce liquid packaging paperboard base paper.
[0059] Preferably, the amount of high-stability cationic lignin rosin sizing agent added in step (4) is 10 to 30 kg per ton of pulp.
[0060] Preferably, the basis weight of the liquid packaging paperboard in step (4) is 80 to 200 g / m 2 .
[0061] Specifically, the relevant preparation and detection are as follows:
[0062] The lignin in the present invention can be purchased from Shanghai McLean Biochemical Technology Co., Ltd., with the item number L849279; the rosin in the present invention can be purchased from Shanghai McLean Biochemical Technology Co., Ltd., with the item number C832364. Epichlorohydrin in the present invention can be purchased from Shanghai McLean Biochemical Technology Co., Ltd., with the item number E808937. Triethylamine in the present invention can be purchased from Shanghai McLean Biochemical Technology Co., Ltd., with the item number T818772. Cationic polyacrylamide in the present invention can be purchased from Shanghai McLean Biochemical Technology Co., Ltd., with the item number P875616. Nonionic polyacrylamide in the present invention can be purchased from Shanghai McLean Biochemical Technology Co., Ltd., with the item number P821239. Aluminum sulfate in the present invention can be purchased from Shanghai McLean Biochemical Technology Co., Ltd., with the item number A801783.
[0063] Example 1
[0064] A method for preparing a cationic lignin rosin sizing agent, the method comprising the following steps:
[0065] (1) Lignin classification:
[0066] A certain amount of lignin was weighed and mixed with a 95% ethanol solution, and stirred for 2 hours at room temperature (speed of 400 rpm). Subsequently, the insoluble part and the soluble part were separated by vacuum filtration. The soluble part (lignin with a molecular weight distribution range of less than 3000 g / mol, denoted as L 95) of ethanol was recovered by rotary evaporation, and the insoluble part was dried for later use. The insoluble part of the 95% ethanol solution was repeated with the 70% ethanol solution. Subsequently, the soluble part (lignin with a molecular weight distribution range of 3000-5000 g / mol, denoted as L 70 ) and the insoluble part (lignin with a molecular weight distribution range greater than 5000 g / mol, denoted as L R The ethanol in the dissolved part was recovered by rotary evaporation, and the insoluble part was dried in an oven at 50°C for later use.
[0067] (2) Preparation of lignin cationic surfactant
[0068] 4gL R Mix with 16g of epichlorohydrin in 60ml of 6mol / L sodium hydroxide solution, and stir in a water bath at 65℃ for 5h at a constant temperature of 500rpm. After stirring, filter to obtain a solid product. Mix the solid product with 16g of triethylamine in 60ml of 0.3mol / L sodium hydroxide solution. After the reaction is completed, adjust the pH value of the solution to acidity with hydrochloric acid; after filtering, wash the obtained solid with deionized water, repeat this process until the solid is neutral, then dry the product at 50℃ for 12h, and finally obtain the lignin cationic surfactant LCS after grinding. R .
[0069] (3) Preparation of cationic lignin rosin sizing agent
[0070] Heat and melt the solid rosin into a uniform rosin liquid for later use; LCS R , cationic polyacrylamide (CPAM) and nonionic polyacrylamide (NPAM) were dispersed in deionized water under constant magnetic stirring conditions of 80 °C and 500 rpm to obtain a uniform emulsifier. The emulsifier was mixed with rosin liquid and homogenized at a high pressure of 60 MPa for 5 min to obtain LCDRS R Among them, LCS R , the mass ratio of CPAM, NPAM, rosin liquid, and deionized water is 1.5:1.5:0.75:100:100;
[0071] The method for making liquid packaging paperboard base paper using the cationic lignin rosin sizing agent comprises the following steps:
[0072] Select softwood with a beating degree of 30°SR and mix it with mechanical pulp at a mass ratio of 1:2. Use aluminum sulfate to adjust the pulp pH to 5.5, and then add LCDRS R , the paper is made on a fast paper former, the basis weight of the liquid packaging paperboard is 160g / m 2 .
[0073] Example 2
[0074] A method for preparing a cationic lignin rosin sizing agent, the method comprising the following steps:
[0075] (1) Lignin classification:
[0076] A certain amount of lignin was weighed and mixed with a 95% ethanol solution, and stirred for 2 hours at room temperature (speed of 400 rpm). Subsequently, the insoluble part and the soluble part were separated by vacuum filtration. The soluble part (lignin with a molecular weight distribution range of less than 3000 g / mol, denoted as L 95 ) of ethanol was recovered by rotary evaporation, and the insoluble part was dried for later use. The insoluble part of the 95% ethanol solution was repeated with the 70% ethanol solution. Subsequently, the soluble part (lignin with a molecular weight distribution range of 3000-5000 g / mol, denoted as L 70 ) and the insoluble part (lignin with a molecular weight distribution range greater than 5000 g / mol, denoted as L R The ethanol in the dissolved part was recovered by rotary evaporation, and the insoluble part was dried in an oven at 50°C for later use.
[0077] (2) Preparation of lignin cationic surfactant
[0078] 4gL 95 Mix with 16g of epichlorohydrin in 60ml of 6mol / L sodium hydroxide solution, and stir in a water bath at 65℃ for 5h at a constant temperature of 500rpm. After stirring, filter to obtain a solid product. Mix the solid product with 16g of triethylamine in 60ml of 0.3mol / L sodium hydroxide solution. After the reaction is completed, adjust the pH value of the solution to acidity with hydrochloric acid; after filtering, wash the obtained solid with deionized water, repeat this process until the solid is neutral, then dry the product at 50℃ for 12h, and finally obtain the lignin cationic surfactant LCS after grinding. 95 .
[0079] (3) Preparation of cationic lignin rosin sizing agent
[0080] Heat and melt the solid rosin into a uniform rosin liquid for later use; LCS 95 , cationic polyacrylamide (CPAM) and nonionic polyacrylamide (NPAM) were dispersed in deionized water under constant magnetic stirring conditions of 80 °C and 500 rpm to obtain a uniform emulsifier. The emulsifier was mixed with rosin liquid and homogenized at a high pressure of 60 MPa for 5 min to obtain LCDRS 95 Among them, LCS 95, the mass ratio of CPAM, NPAM, rosin liquid, and deionized water is 1.5:1.5:0.75:100:100;
[0081] The method for making liquid packaging paperboard base paper using the cationic lignin rosin sizing agent comprises the following steps:
[0082] Select softwood with a beating degree of 30°SR and mix it with mechanical pulp at a mass ratio of 1:2. Use aluminum sulfate to adjust the pulp pH to 5.5, and then add LCDRS 95 , the paper is made on a fast paper former, the basis weight of the liquid packaging paperboard is 160g / m 2 .
[0083] Example 3
[0084] A method for preparing a cationic lignin rosin sizing agent, the method comprising the following steps:
[0085] (1) Lignin classification:
[0086] A certain amount of lignin was weighed and mixed with a 95% ethanol solution, and stirred for 2 hours at room temperature (speed of 400 rpm). Subsequently, the insoluble part and the soluble part were separated by vacuum filtration. The soluble part (lignin with a molecular weight distribution range of less than 3000 g / mol, denoted as L 95 ) of ethanol was recovered by rotary evaporation, and the insoluble part was dried for later use. The insoluble part of the 95% ethanol solution was repeated with the 70% ethanol solution. Subsequently, the soluble part (lignin with a molecular weight distribution range of 3000-5000 g / mol, denoted as L 70 ) and the insoluble part (lignin with a molecular weight distribution range greater than 5000 g / mol, denoted as L R The ethanol in the dissolved part was recovered by rotary evaporation, and the insoluble part was dried in an oven at 50°C for later use.
[0087] (2) Preparation of lignin cationic surfactant
[0088] 4gL 70 Mix with 16g of epichlorohydrin in 60ml of 6mol / L sodium hydroxide solution, and stir in a water bath at 65℃ for 5h at a constant temperature of 500rpm. After stirring, filter to obtain a solid product. Mix the solid product with 16g of triethylamine in 60ml of 0.3mol / L sodium hydroxide solution. After the reaction is completed, adjust the pH value of the solution to acidity with hydrochloric acid; after filtering, wash the obtained solid with deionized water, repeat this process until the solid is neutral, then dry the product at 50℃ for 12h, and finally obtain the lignin cationic surfactant LCS after grinding.70 .
[0089] (3) Preparation of cationic lignin rosin sizing agent
[0090] Heat and melt the solid rosin into a uniform rosin liquid for later use; LCS 70 , cationic polyacrylamide (CPAM) and nonionic polyacrylamide (NPAM) were dispersed in deionized water under constant magnetic stirring conditions of 80 °C and 500 rpm to obtain a uniform emulsifier. The emulsifier was mixed with rosin liquid and homogenized at a high pressure of 60 MPa for 5 min to obtain LCDRS 70 Among them, LCS 70 , the mass ratio of CPAM, NPAM, rosin liquid, and deionized water is 1.5:1.5:0.75:100:100;
[0091] The method for making liquid packaging paperboard base paper using the cationic lignin rosin sizing agent comprises the following steps:
[0092] Select softwood with a beating degree of 30°SR and mix it with mechanical pulp at a mass ratio of 1:2. Use aluminum sulfate to adjust the pulp pH to 5.5, and then add LCDRS 70 , the paper is made on a fast paper former, the basis weight of the liquid packaging paperboard is 160g / m 2 .
[0093] Figure 1 The figure is a comparison of the molecular weight and polydispersity index (PDI) of different fractions of lignin in Examples 1-3 of the present invention. The molecular weight of lignin was detected by gel chromatography. The detection conditions were: DMSO as the eluent, temperature 40°C, flow rate 1 mL / min.
[0094] Figure 2 The two-dimensional NMR comparison diagram of different fractions of lignin in Examples 1-3 of the present invention. The detection method is: 50 mg of the sample to be tested (pre-dried) is dispersed in 0.6 mL of DMSO-d6 reagent, ultrasonically treated to fully dissolve it, and then transferred to a clean NMR tube and the sample is detected by the corresponding HSQC program.
[0095] Figure 3 The comparison chart of the particle sizes of cationic lignin rosin sizing agents of different sizes in Examples 1-3 of the present invention is as follows: the concentration of the cationic lignin rosin sizing agent emulsion prepared by different grades of lignin is 5 mg / mL, an appropriate amount of sample is added to the sample pool, and the particle size is measured by a Malvern particle size analyzer at room temperature of 25°C, and the number of measurements is set to three times.
[0096] Figure 4This is a comparison chart of the Zeta potential of cationic lignin rosin sizing agents of different sizes in Examples 1-3 of the present invention. The detection method is: configure the cationic lignin rosin sizing agent emulsion with different grades of lignin to a concentration of 5 mg / mL, take an appropriate amount of sample and add it to the sample pool, use a Malvern particle size analyzer to measure at room temperature 25°C, and set the measurement number to three times.
[0097] like Figure 1 It can be seen that the lignin L in Example 1 R The molecular weight of lignin is the highest, which is Mw = 8708 g / mol. When the molecular weight of lignin increases, the number of reaction sites between lignin and subsequent epichlorohydrin also increases, which helps to increase the yield of lignin surfactant.
[0098] Depend on Figure 2 It can be seen that for all lignin fractions, the chemical shift range of C / H = 50-90 / 3.0-4.8 is the characteristic region of aliphatic CO, among which the signal of methoxy (C / H = 56.3 / 3.75) is the strongest in this region. As the ethanol concentration decreases, it is found that the signal intensity of β-5 and β-β structures decreases significantly, while the signal of β-O-4 structure gradually increases. In addition, hydroxybenzene lignin can be removed during the ethanol / water fractionation process. The above results show that low molecular weight lignin is easily dissolved in the solvent, while high molecular weight lignin is relatively difficult (such as L R ). Therefore, using different concentrations of ethanol can achieve the classification of lignin raw materials into fractions with different molecular weights and functional groups, further improving the uniformity of lignin.
[0099] according to Figure 3 The particle size of the emulsion in Example 1 is shown in Table 1. The particle size of the emulsion in Example 1 is larger, but still nanoparticles, and the PDI value is lower, indicating that the emulsion has the best stability. In addition, the Zeta potential of different cationic lignin rosin sizing agent emulsions was tested. The results are shown in Table 1. Figure 4 As shown. Zeta potential is a measure of the strength of mutual repulsion or attraction between particles. The smaller the molecule or dispersed particle, the higher the absolute value of the Zeta potential, and the more stable the system, that is, the dissolution or dispersion can resist aggregation. The quaternary ammonium modified lignin surfactant makes the Zeta potential of the emulsion positive. In Example 1, the absolute value of the Zeta potential of the emulsion is greater than 40mV, the particles tend to repel each other, and it is not easy to coalesce, etc., and the emulsion has good stability.
[0100] Comparative Example 1
[0101] Select softwood with a beating degree of 30°SR and mix it with mechanical pulp at a mass ratio of 1:2. Use aluminum sulfate to adjust the pulp pH to 5.5, and then make sheets on a fast paper former. The basis weight of the liquid packaging paperboard base paper is 160g / m 2.
[0102] Comparative Example 2
[0103] A rosin size in a novel cationic rosin sizing agent disclosed in patent application number 201710694208.1 was selected as comparative example 2, and the same quantitative amount was used to carry out the papermaking experiment and the hydrophobicity detection experiment. The remaining papermaking steps were the same as those in Example 1.
[0104] Comparative Example 3 (Unclassified Lignin)
[0105] Mix 4g of lignin and 16g of epichlorohydrin in 60ml of 6mol / L sodium hydroxide solution, and stir in a water bath at 65°C for 5h at a constant temperature of 500rpm. After stirring, filter to obtain a solid product. Mix the solid product with 16g of triethylamine in 60ml of 0.3mol / L sodium hydroxide solution. After the reaction is completed, adjust the pH value of the solution to acidity with hydrochloric acid; after filtering, wash the obtained solid with deionized water, repeat this process until the solid is neutral, then dry the product at 50°C for 12h, and finally obtain the lignin cationic surfactant LCS after grinding. O .
[0106] Heat and melt the solid rosin into a uniform rosin liquid for later use; LCS O , cationic polyacrylamide (CPAM) and nonionic polyacrylamide (NPAM) were dispersed in deionized water under constant magnetic stirring conditions of 80 °C and 500 rpm to obtain a uniform emulsifier. The emulsifier was mixed with rosin liquid and homogenized at a high pressure of 60 MPa for 5 min to obtain LCDRS O Among them, LCS O , the mass ratio of CPAM, NPAM, rosin liquid, and deionized water is 1.5:1.5:0.75:100:100;
[0107] The method for making liquid packaging paperboard base paper using the cationic lignin rosin sizing agent comprises the following steps:
[0108] Select softwood with a beating degree of 30°SR and mix it with mechanical pulp at a mass ratio of 1:2. Use aluminum sulfate to adjust the pulp pH to 5.5, and then add LCDRS O , the paper is made on a fast paper former, the basis weight of the liquid packaging paperboard is 160g / m 2 .
[0109] Comparative Example 4 (without addition of lignin)
[0110] Heat and melt solid rosin into uniform rosin liquid for use; disperse cationic polyacrylamide (CPAM) and nonionic polyacrylamide (NPAM) in deionized water, and stir at 80°C and 500rpm under constant magnetic stirring to obtain a uniform emulsifier. Mix the emulsifier with the rosin liquid, and homogenize for 5 minutes under a high pressure of 60MPa to obtain a rosin sizing agent. The mass ratio of CPAM, NPAM, rosin liquid, and deionized water is 1.5:0.75:100:100;
[0111] The method for making base paper for liquid packaging paperboard using the above-mentioned rosin sizing agent comprises the following steps:
[0112] Select softwood with a beating degree of 30°SR and mix it with mechanical pulp at a mass ratio of 1:2. Use aluminum sulfate to adjust the pulp pH to 5.5, then add rosin sizing agent, and make sheets on a fast paper former. The basis weight of liquid packaging paperboard is 160g / m 2 .
[0113] The Cobb value of the cationic lignin rosin sizing agent prepared in Example 1-3 was compared. The test results are as follows: Figure 5 The test method is as follows: the Cobb value of paper is measured according to the standard GB / T1540-2002 using a 61-67 type automatic Cobb value tester (TMI, USA).
[0114] The contact angles of the cationic lignin rosin sizing agents prepared in Examples 1-3 were compared. The test results are as follows: Figure 6 The test method is as follows: The contact angle is measured according to the standard ISO / TS14778:2021 using a PGX dynamic contact angle meter (FIBRO, Sweden).
[0115] The tensile index of the cationic lignin rosin sizing agent prepared in Example 1-3 was compared, and the test results were as follows: Figure 7 The test method is as follows: the tensile index is measured and calculated according to QB / T1053-2004 using a 066 type tensile strength instrument (L&W, Sweden).
[0116] Cobb value and contact angle are usually used to characterize the ability of paper or paperboard surface to resist liquid penetration. The smaller the Cobb value, the better the hydrophobicity of the paperboard. Figure 5 As shown, the Cobb value of the paperboard made in Example 1 is 20.53 g / m 2 , which is lower than the comparative example 4 (24.81 g / m 2 ) and Comparative Example 3 (23.30 g / m 2 ). The larger the contact angle, the better the hydrophobicity of the paperboard. Figure 6As shown in the figure, the contact angle of the paperboard produced in Example 1 is 136.2°, which is higher than that of Comparative Example 4 (128.4°) without adding lignin and Comparative Example 3 (129.1°) with adding unfractionated lignin. This indicates that: (1) the addition of lignin can improve the hydrophobicity of the rosin sizing agent; (2) after the lignin is graded, the increase in molecular weight can further improve the hydrophobicity of the sizing agent.
[0117] Strength performance test results are as follows Figure 7 As shown, the tensile index of Example 1 is 29.71 N·m / g, the tensile index of Example 2 is 26.43 N·m / g, and the tensile index of Example 3 is 27.11 N·m / g. The strength performance of Examples 1-3 is better than that of Comparative Example 4 (21.56 N·m / g) without adding lignin and Comparative Example 3 (25.85 N·m / g) with adding unfractionated lignin. This may be because the lignin classification process can remove the low molecular weight lignin part, while the high molecular weight lignin has more reaction sites. Therefore, in the process of quaternary ammonium modification of high molecular weight lignin, more quaternary ammonium groups can be introduced into lignin, so that more lignin is adsorbed on the surface of rosin particles. Finally, the sizing agent prepared by high molecular weight lignin also has the best strength performance.
[0118] At the same time, by comparing Examples 1-3, Comparative Example 2 and Comparative Example 4, it can also be seen that the rosin in the present invention and the classified lignin have a synergistic effect and can synergistically improve the relevant properties of the prepared sizing agent.
[0119] Therefore, it can be seen that the highly stable cationic lignin rosin sizing agent prepared in the method of the present invention can effectively improve the hydrophobicity and strength properties of the finished paper.
[0120] In summary, the present invention discloses a method for preparing a highly stable cationic lignin rosin sizing agent. The prepared sizing agent has good stability, can improve the hydrophobicity and strength properties of paper, and can be applied to liquid packaging paperboard.
[0121] Although the embodiments of the present invention are disclosed for illustrative purposes, those skilled in the art will appreciate that various substitutions, changes and modifications are possible without departing from the spirit and scope of the present invention and the appended claims. Therefore, the scope of the present invention is not limited to the contents disclosed in the embodiments.
Claims
1. A method for making liquid packaging paperboard base paper using a high-stability cationic lignin rosin sizing agent, characterized in that: The steps include: Adding high-stability cationic lignin rosin sizing agent emulsion into pulp to make liquid packaging paperboard base paper; The preparation method of the high-stability cationic lignin rosin sizing agent comprises the following steps: (1) Weighing lignin powder, mixing it with an ethanol solution with a mass concentration of 95%, stirring, letting it stand, and filtering to obtain an insoluble part and a soluble part, wherein the lignin with a molecular weight distribution range of less than 3000 g / mol is the soluble part, and the ethanol in the soluble part is recovered by rotary evaporation, and the insoluble part is dried for later use; repeating the above steps with the insoluble part of the ethanol solution with a mass concentration of 95% and continuing to mix it with the ethanol solution with a mass concentration of 70%; Subsequently, the soluble part and the insoluble part were separated by vacuum filtration, wherein the soluble part was lignin with a molecular weight distribution range of 3000-5000 g / mol, and the insoluble part was lignin with a molecular weight distribution range of more than 5000 g / mol. The ethanol in the soluble part was recovered by rotary evaporation, and the insoluble part was dried in an oven at 50°C for later use; (2) Mixing fractionated lignins of different molecular weights, i.e., lignin with a molecular weight distribution range of more than 5000 g / mol, lignin with a molecular weight distribution range of 3000-5000 g / mol, and lignin with a molecular weight distribution range of less than 3000 g / mol, with epichlorohydrin in a strong alkaline solution, stirring, and filtering to obtain a solid product; The solid product is mixed with triethylamine in a dilute alkaline solution, and after the reaction is completed, the pH value of the solution is adjusted to acidic with hydrochloric acid; after filtering, the obtained solid is washed with deionized water, and this process is repeated until the solid is neutral, and then the product is dried under conditions; (3) heating and melting solid rosin into a uniform rosin liquid; dispersing the product of step (2) with cationic polyacrylamide and nonionic polyacrylamide in deionized water, and stirring to obtain a uniform emulsifier; mixing the emulsifier and rosin liquid and homogenizing under high pressure to obtain a high-stability cationic lignin rosin sizing agent; In step (2), the mass ratio of lignin, epichlorohydrin and triethylamine is 1:1-5:1-5; The strong alkaline solution in step (2) is a 3-7 mol / L sodium hydroxide solution; The stirring conditions in step (2) are: 50-80°C, 500-1000 rpm, 2-5h; The dilute alkaline solution in step (2) is a 0.1-1 mol / L sodium hydroxide solution; In step (3), the mass ratio of the product, cationic polyacrylamide, nonionic polyacrylamide, rosin liquid and deionized water is 0.5-5:0.5-5:0.5-5:50-100: 50-100; The conditions of high pressure homogenization in step (3) are: 20-60 MPa, 5-30 min.
2. The method according to claim 1, characterized in that: The stirring time in step (1) is 10 to 120 min.
3. The method according to claim 1, characterized in that: The drying conditions in step (2) are: 30~80°C, 8~20 h.
4. The method according to claim 1, characterized in that: The stirring conditions in step (3) are: 50~100°C, 500~2000 rpm.
5. The method according to claim 1, characterized in that: A high-stability cationic lignin rosin sizing agent emulsion is added into the pulp, wherein the addition amount of the high-stability cationic lignin rosin sizing agent is 10-30 kg / ton of pulp.
6. The method according to any one of claims 1 to 5, characterized in that: The basis weight of liquid packaging paperboard is 80~200 g / m 2 .
Citation Information
Patent Citations
Grading method of lignin
CN106750362A
Hard polyurethane material reinforced by modified lignin and preparation method thereof
CN107383307A
Cationic rosin emulsion neutral-alkaline sizing agent and preparation method thereof
CN107630387A
Method for comprehensively utilizing lignin
CN107698779A
Method for grading lignin by gamma-valerolactone / water system
CN108822304A