A method for improving the poor sintering bubbles of DCB substrate of thin ceramic sheets

By designing the opening pad plate and the sintering fixture for sticking porcelain strips, the problem of poor sintering bubbles between thin porcelain pieces and copper pieces is solved, and the uniform flow of copper oxide eutectic liquid and the improvement of sintering quality is achieved.

CN116387163BActive Publication Date: 2024-11-05SHANGHAI FULLERHUA SEMICON TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310253500.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-03-16
Publication Date
2024-11-05
Estimated Expiration
2043-03-16

AI Technical Summary

Technical Problem

In the prior art, bubble problems often occur during the sintering process between thin porcelain sheets and copper sheets, especially when the thickness of the ceramic sheet is less than 0.38 mm, resulting in poor sintering.

Method used

Design a sintering fixture with openings at both ends of the pad plate and sticking porcelain strips on both sides to reduce the contact area of ​​the pad plate to the porcelain piece, so that the porcelain piece naturally deforms in the middle, ensuring that the copper oxide eutectic liquid flows evenly, thereby reducing the The generation of bubbles.

Benefits of technology

By reducing the unnaturally deformed by the pad plate on the ceramic sheet, the uniform flow of the copper oxide eutectic liquid during the sintering of the ceramic sheet and the copper sheet is achieved, which significantly reduces the generation of sintered bubbles and improves the quality of the thin DCB substrate.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116387163B_ABST
    Figure CN116387163B_ABST
Patent Text Reader

Abstract

The present invention relates to the field of semiconductor technology. A method for improving the poor sintering bubbles of a DCB substrate of a thin ceramic sheet, comprising the following steps: Step 1, pasting two parallel ceramic strips on the upper left and right sides of a pad to form a sintering jig; notches are provided at both the front and rear ends of the pad; Step 2, placing the sintering jig on a conveyor belt, and the pad of the sintering jig contacts the conveyor belt; Step 3, placing the ceramic sheet to be sintered and the copper foil on the sintering jig in sequence, with the thickness of the ceramic sheet being less than 0.38 mm; Step 4, sintering. The present invention designs the pad to be open at both the front and rear ends, so that the ceramic sheet contacts the pad only in the middle, and only at the edges at both ends in the length direction. By reducing the contact area, the influence of the pad on the sintering of the DCB substrate is reduced, so that the deformation of the thin ceramic sheet is in a natural deformation state, and the cuprous oxide eutectic liquid flows evenly, thereby reducing the poor sintering bubbles.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of semiconductor technology, in particular to a sintering method for a copper-clad ceramic substrate. Background Art

[0002] Copper clad ceramic substrate (DCB substrate) is made by wetting the copper sheet and alumina ceramic surface in contact with each other with cuprous oxide eutectic liquid, so that the two are firmly combined together, thereby making a DCB substrate.

[0003] In the current production process, when the thickness of the ceramic sheet of the DCB substrate is thin (ceramic thickness < 0.38mm), there are more sintering bubbles between the ceramic sheet and the copper sheet, and most of them are distributed at both ends of the length direction of the product. The reason is that when the ceramic sheet and the copper sheet of the DCB substrate are sintered, according to the process requirements, a pad of the same size as the ceramic sheet must be placed under the ceramic sheet. Under high temperature, the thinner ceramic sheet will produce a certain deformation, and the pad makes the thin ceramic sheet deform in an unnatural deformation state. When the cuprous oxide eutectic liquid between the ceramic and copper gradually flows from the middle to the two ends, the unnatural deformation of the thin ceramic sheet will cause the eutectic liquid at both ends to be unevenly distributed, thereby generating more bubbles.

[0004] Currently, there is a lack of methods to solve the problem of poor sintering bubbles between thin ceramic sheets with a ceramic thickness of less than 0.38 mm and copper sheets. Summary of the invention

[0005] In view of the problems existing in the prior art, the present invention provides a method for improving the poor sintering bubbles of a DCB substrate of a thin ceramic sheet, so as to solve at least one of the above technical problems.

[0006] In order to achieve the above object, the present invention provides a method for improving the poor sintering bubbles of a DCB substrate of a thin ceramic sheet, characterized in that it comprises the following steps:

[0007] Step 1: stick two parallel porcelain strips on the upper left and right sides of the pad to form a sintering fixture;

[0008] The backing plate is provided with notches at both the front and rear ends;

[0009] Step 2, placing the sintering jig on the conveyor belt, with the backing plate of the sintering jig contacting the conveyor belt;

[0010] Step 3, placing the ceramic sheet to be sintered and the copper foil on the sintering fixture in sequence, wherein the thickness of the ceramic sheet is less than 0.38 mm;

[0011] Step 4: sintering.

[0012] The present invention designs the pad to be open at both ends, so that the ceramic sheet contacts the pad only in the middle and at both ends in the length direction only at the edges. The contact area is reduced to reduce the influence of the pad on the sintering of the DCB substrate, so that the deformation of the thin ceramic sheet is in a natural deformation state, and the cuprous oxide eutectic liquid flows evenly, thereby reducing sintering bubbles.

[0013] Further preferably, the ceramic strip is adhered to the pad by organic glue.

[0014] Further preferably, the length of the ceramic strip in the front-to-back direction is equal to the length of the pad in the front-to-back direction.

[0015] Further preferably, the pad has a length of 190 mm, a width of 138 mm, and a thickness of 1 mm.

[0016] Further preferably, the length of the ceramic strip is 190 mm, the width is 3 mm, and the thickness is 1 mm.

[0017] Further preferably, the left side edge of the ceramic strip located on the left side is aligned with the left side edge of the pad;

[0018] The right side edge of the porcelain strip located on the right side is aligned with the right side edge of the pad.

[0019] Further preferably, the pad is H-shaped, and includes two strip structures arranged on the left and right and a connecting portion connecting the strip structures;

[0020] The width of the strip structure in the left-right direction is greater than the width of the ceramic strip in the left-right direction, and is not less than 1.5 times the width of the ceramic strip in the left-right direction, and is not greater than 3 times the width of the magnetic strip in the left-right direction;

[0021] The length of the connecting portion in the front-to-back direction is not less than 1 / 11 of the length of the pad in the front-to-back direction, and is not greater than 1 / 8 of the length of the pad in the front-to-back direction.

[0022] Further preferably, the length of the connecting portion in the front-to-back direction is 20 mm.

[0023] Further preferably, the notch is in a U-shape with the opening facing outwards;

[0024] The length of the notch is 85 mm, the width is 126 mm, and the corners of the notch are rounded with a radius of 15 mm.

[0025] Further preferably, in step 2, the length direction of the pad is parallel to the length direction of the conveyor belt.

[0026] Further preferably, the raw material of the backing plate includes 96% by mass of Al2O3 ceramic, 1.5%-2.3% by mass of SiO2, and the remainder is magnesium and calcium;

[0027] The raw materials of the ceramic strip include 96% by mass of Al2O3 ceramics, 1.5%-2.3% by mass of SiO2, and the remainder is magnesium and calcium.

[0028] Further preferably, in step 4, the sintering fixture passes through three temperature rising zones, four constant temperature zones and three temperature falling zones in sequence;

[0029] The three heating zones are set at temperatures between 755°C and 765°C, 850°C and 860°C, and 1030°C and 1040°C, respectively;

[0030] The total length of the heating zone is 1000-1100 mm; the time for the sintering fixture to pass through the heating zone is 9-13 minutes.

[0031] The passing time of the three heating zones is 3-4.5min, 3-4.5min, and 3-4.5min respectively.

[0032] The temperature of the four constant temperature zones is set between 1070°C and 1075°C; the total length of the constant temperature zones is 1300 to 1500 mm; and the time for the sintering fixture to pass through the constant temperature zones is 14 to 18 minutes.

[0033] The three cooling zones are set at temperatures between 1025℃~1035℃, 970℃~980℃, and 920℃~930℃ respectively;

[0034] The total length of the cooling zone is 1000-1100 mm, and the time for the sintering fixture to pass through the cooling zone is 9-13 minutes. The passing time of the three cooling zones is 3-4.5 minutes, 3-4.5 minutes, and 3-4.5 minutes, respectively.

[0035] The conveying rate of the sintering fixture is 80-85 mm / min. BRIEF DESCRIPTION OF THE DRAWINGS

[0036] Figure 1 A schematic diagram of the structure of a sintering jig according to a specific embodiment 1 of the present invention;

[0037] Figure 2 It is a schematic structural diagram of the sintering fixture of the specific embodiment 1 of the present invention from another perspective.

[0038] Among them: 1 is a backing plate, 2 is a porcelain strip, and 11 is a gap. DETAILED DESCRIPTION

[0039] The present invention will be further described below in conjunction with the accompanying drawings.

[0040] See also Figure 1 as well as Figure 2 , Specific embodiment 1, a method for improving the poor sintering bubbles of a DCB substrate of a thin ceramic sheet, comprising the following steps:

[0041] Step 1: Paste two parallel ceramic strips 2 on the upper left and right sides of the backing plate 1 to form a sintering fixture; and the ceramic strips 2 are pasted on the backing plate 1 by organic glue.

[0042] Notches 11 are provided at both the front and rear ends of the pad 1;

[0043] Step 2: Place the sintering jig on the conveyor belt, with the pad of the sintering jig in contact with the conveyor belt; the length direction of the pad 1 is parallel to the length direction of the conveyor belt.

[0044] Step three, placing the ceramic sheet to be sintered and the copper foil on the sintering fixture in sequence, the thickness of the ceramic sheet is less than 0.38 mm; the thickness of the ceramic sheet is greater than or equal to 0.25 mm.

[0045] Step 4: sintering.

[0046] The present invention designs the backing plate 1 to be open at both ends, so that the ceramic piece contacts the backing plate 1 only in the middle and only at the edges at both ends in the length direction. By reducing the contact area, the influence of the backing plate 1 on the sintering of the DCB substrate is reduced, so that the thin ceramic piece is deformed in a natural deformation state, and the cuprous oxide eutectic liquid flows evenly, thereby reducing sintering bubbles. The ceramic piece to be sintered is placed on top of the ceramic strip.

[0047] The length of the porcelain strip 2 in the front-to-back direction is equal to the length of the pad 1 in the front-to-back direction.

[0048] The length of the pad 1 is 190 mm, the width is 138 mm, and the thickness is 1 mm.

[0049] The length of the porcelain strip 2 is 190 mm, the width is 3 mm, and the thickness is 1 mm.

[0050] The left side edge of the ceramic strip 2 located on the left side is aligned with the left side edge of the pad 1; the right side edge of the ceramic strip 2 located on the right side is aligned with the right side edge of the pad 1.

[0051] The pad 1 is H-shaped, and includes two strip structures arranged on the left and right and a connecting portion connecting the strip structures; the width of the strip structure in the left and right direction is greater than the width of the ceramic strip 2 in the left and right direction, and is not less than 1.5 times the width of the ceramic strip 2 in the left and right direction, and is not greater than 3 times the width of the magnetic strip in the left and right direction; the length of the connecting portion in the front-to-back direction is not less than 1 / 11 of the length of the pad 1 in the front-to-back direction, and is not greater than 1 / 8 of the length of the pad 1 in the front-to-back direction. Preferably, the length of the connecting portion in the front-to-back direction is 20 mm.

[0052] The notch 11 is in a U-shape with its opening facing outwards; the notch is 85 mm long and 126 mm wide, and the corners of the notch are rounded with a radius of 15 mm.

[0053] The raw materials of the pad 1 include 96% by mass AL2O3 ceramics, 1.5%-2.3% by mass SiO2, and the remainder are magnesium and calcium; the raw materials of the ceramic strip 2 include 96% by mass AL2O3 ceramics, 1.5%-2.3% by mass SiO2, and the remainder are magnesium and calcium.

[0054] In step 4, the sintering fixture passes through three temperature rising zones, four constant temperature zones and three temperature falling zones in sequence;

[0055] The three heating zones are set at temperatures between 755°C and 765°C, 850°C and 860°C, and 1030°C and 1040°C, respectively;

[0056] The total length of the heating zone is 1000-1100 mm; the time for the sintering fixture to pass through the heating zone is 9-13 minutes;

[0057] The transit time of the three heating zones is 3-4.5min, 3-4.5min, and 3-4.5min, respectively;

[0058] The temperature of the four constant temperature zones is set between 1070℃ and 1075℃; the total length of the constant temperature zones is 1300-1500mm; the time for the sintering fixture to pass through the constant temperature zones is 14-18min;

[0059] The three cooling zones are set at temperatures between 1025℃~1035℃, 970℃~980℃, and 920℃~930℃ respectively;

[0060] The total length of the cooling zone is 1000-1100mm; the time for the sintering fixture to pass through the cooling zone is 9-13min. The passing time of the three cooling zones is 3-4.5min, 3-4.5min, and 3-4.5min respectively;

[0061] The conveying rate of the sintering fixture is 80-85 mm / min.

[0062] Comparative Example 1:

[0063] The sintering is carried out in the manner of the background technology. A pad matching the size of the ceramic piece is placed on a conveyor belt to support the ceramic piece and the copper piece for sintering. During sintering, three heating zones, four constant temperature zones and three cooling zones are passed in sequence;

[0064] The three heating zones are set at temperatures between 750°C and 760°C, 845°C and 855°C, and 1025°C and 1035°C respectively;

[0065] The total length of the heating zone is 1000-1100 mm; the time for the sintering fixture to pass through the heating zone is 10-15 minutes;

[0066] The transit time of the three heating zones is 3.5-5.5min, 3.5-5.5min, and 3.5-5.5min, respectively;

[0067] The temperature of the four constant temperature zones is set between 1065℃ and 1070℃; the total length of the constant temperature zones is 1300-1500mm; the time for the sintering fixture to pass through the constant temperature zones is 15-20min;

[0068] The three cooling zones are set at temperatures between 1020℃~1030℃, 965℃~975℃, and 915℃~925℃ respectively;

[0069] The total length of the cooling zone is 1000-1100mm; the time for the sintering fixture to pass through the cooling zone is 10-15min. The passing time of the three cooling zones is 3.5-5.5min, 3.5-5.5min, and 3.5-5.5min respectively;

[0070] The conveying rate of the sintering fixture is 75-80 mm / min.

[0071] Comparative Example 2:

[0072] The sintering is performed in the manner of the background technology. A pad matching the size of the ceramic sheet is placed on a conveyor belt to support the ceramic sheet and the copper sheet for sintering.

[0073] The sintering fixture passes through three temperature rising zones, four constant temperature zones and three temperature falling zones in sequence;

[0074] The three heating zones are set at temperatures between 755°C and 765°C, 850°C and 860°C, and 1030°C and 1040°C, respectively;

[0075] The total length of the heating zone is 1000-1100 mm; the time for the sintering fixture to pass through the heating zone is 9-13 minutes;

[0076] The transit time of the three heating zones is 3-4.5min, 3-4.5min, and 3-4.5min, respectively;

[0077] The temperature of the four constant temperature zones is set between 1070℃ and 1075℃; the total length of the constant temperature zones is 1300-1500mm; the time for the sintering fixture to pass through the constant temperature zones is 14-18min;

[0078] The three cooling zones are set at temperatures between 1025℃~1035℃, 970℃~980℃, and 920℃~930℃ respectively;

[0079] The total length of the cooling zone is 1000-1100mm; the time for the sintering fixture to pass through the cooling zone is 9-13min. The passing time of the three cooling zones is 3-4.5min, 3-4.5min, and 3-4.5min respectively;

[0080] The conveying rate of the sintering fixture is 80-85 mm / min.

[0081] Comparative Example 3: The solution of the specific embodiment 1 of the present invention is adopted, except that the sintering process adopts the traditional sintering process:

[0082] During sintering, it passes through three temperature rising zones, four constant temperature zones and three temperature falling zones in sequence;

[0083] The three heating zones are set at temperatures between 750°C and 760°C, 845°C and 855°C, and 1025°C and 1035°C respectively;

[0084] The total length of the heating zone is 1000-1100 mm; the time for the sintering fixture to pass through the heating zone is 10-15 minutes;

[0085] The transit time of the three heating zones is 3.5-5.5min, 3.5-5.5min, and 3.5-5.5min, respectively;

[0086] The temperature of the four constant temperature zones is set between 1065℃ and 1070℃; the total length of the constant temperature zones is 1300-1500mm; the time for the sintering fixture to pass through the constant temperature zones is 15-20min;

[0087] The three cooling zones are set at temperatures between 1020℃~1030℃, 965℃~975℃, and 915℃~925℃ respectively;

[0088] The total length of the cooling zone is 1000-1100mm; the time for the sintering fixture to pass through the cooling zone is 10-15min. The passing time of the three cooling zones is 3.5-5.5min, 3.5-5.5min, and 3.5-5.5min respectively;

[0089] The conveying rate of the sintering fixture is 75-80 mm / min.

[0090] The performance parameters of the present invention, comparative example 1, comparative example 2, and comparative example 3 are compared as follows:

[0091]

[0092] The above are only preferred embodiments of the present invention. It should be pointed out that, for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principles of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A method for improving the sintering bubble problem of a thin-type DCB substrate, characterized in that: The steps include: Step 1: Glue two parallel porcelain strips on the left and right sides of the backing plate to form a sintering fixture; Notches are provided at both the front and rear ends of the pad; Step 2: placing the sintering jig on a conveyor belt, with the backing plate of the sintering jig in contact with the conveyor belt; Step 3: placing the ceramic sheet to be sintered and the copper foil on the sintering jig in sequence, wherein the thickness of the ceramic sheet is less than 0.38 mm; Step 4, sintering; The ceramic strip is adhered to the backing plate by organic glue; In step 2, the length direction of the pad is parallel to the length direction of the conveyor belt; The length of the porcelain strip in the front-to-back direction is equal to the length of the backing plate in the front-to-back direction; The length of the pad is 190 mm, the width is 138 mm, and the thickness is 1 mm; The length of the porcelain strip is 190 mm, the width is 3 mm, and the thickness is 1 mm; The left side of the porcelain strip on the left is aligned with the left side of the pad; The right side edge of the porcelain strip on the right side is aligned with the right side edge of the pad; The backing plate is H-shaped and includes two strip structures arranged on the left and right and a connecting portion connecting the strip structures; The width of the strip structure in the left-right direction is greater than the width of the porcelain strip in the left-right direction, and is not less than 1.5 times the width of the porcelain strip in the left-right direction, and is not greater than 3 times the width of the porcelain strip in the left-right direction; The length of the connecting portion in the front-to-back direction is not less than 1 / 11 of the length of the backing plate in the front-to-back direction, and not more than 1 / 8 of the length of the backing plate in the front-to-back direction; The length of the connecting portion in the front-to-back direction is 20 mm; The notch is in a U-shape with the opening facing outward; The notch is 85 mm long and 126 mm wide, and the corners of the notch are rounded with a radius of 15 mm; In step 4, the sintering fixture passes through three temperature rising zones, four constant temperature zones and three temperature falling zones in sequence; The three heating zones are set at temperatures between 755℃~765℃, 850℃~860℃, and 1030℃~1040℃ respectively; The total length of the heating zone is 1000-1100 mm; the time for the sintering fixture to pass through the heating zone is 9-13 minutes; The transit time of the three heating zones is 3-4.5 min, 3-4.5 min, and 3-4.5 min, respectively; The temperature of the four constant temperature zones is set between 1070℃ and 1075℃; the total length of the constant temperature zones is 1300-1500mm; the time it takes for the sintering fixture to pass through the constant temperature zones is 14-18 minutes; The three cooling zones are set at temperatures between 1025℃~1035℃, 970℃~980℃, and 920℃~930℃ respectively; The total length of the cooling zone is 1000 to 1100 mm; the time for the sintering fixture to pass through the cooling zone is 9 to 13 minutes.