A high heat-resistant, halogen-free, intrinsically flame-retardant polydicyclopentadiene engineering material and its preparation method

An expandable norborneol-based flame retardant containing phenylphosphonic and piperazine structures, prepared by copolymerization, solves the problems of flammability and decreased mechanical properties of polydicyclopentadiene, and achieves the high-efficiency flame retardant, low-smoke, halogen-free, and non-toxic properties of intrinsically flame-retardant polydicyclopentadiene engineering materials with high heat resistance.

CN116396468BActive Publication Date: 2026-11-17ANHUI UNIVERSITY OF ARCHITECTURE
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202310470532.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-04-27
Publication Date
2026-11-17
Estimated Expiration
2043-04-27

AI Technical Summary

Technical Problem

Polydicyclopentadiene materials are flammable, and when burning, they drip and produce smoke and toxic gases. Furthermore, the uneven dispersion of traditional intumescent flame retardants in the matrix leads to a decline in mechanical properties.

Method used

Highly heat-resistant, halogen-free intrinsically flame-retardant polydicyclopentadiene engineering materials were prepared by copolymerizing an expandable norbornene-based flame retardant containing phenylphosphonyl and piperazine structures with dicyclopentadiene and 1,5-dimethyl-1,5-cyclooctadiene monomers via thermally driven self-propagating technology.

Benefits of technology

The material has excellent flame retardant properties, heat resistance and good balance of rigidity and toughness. The limiting oxygen index reaches 43%, the flame retardant rating reaches UL-94V-0, the tensile strength reaches 131MPa, the elongation at break reaches 48%, and the heat distortion temperature reaches 199℃.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116396468B_ABST
    Figure CN116396468B_ABST
Patent Text Reader

Abstract

This invention discloses a high-heat-resistant, halogen-free, intrinsically flame-retardant polydicyclopentadiene engineering material and its preparation method. This material is produced by copolymerizing an expandable norbornene-based flame retardant monomer containing phenylphosphonic and piperazine structures, along with 1,5-dimethyl-1,5-cyclooctadiene as a copolymer unit, with a dicyclopentadiene monomer. This introduces phosphorus and nitrogen flame-retardant units into the structure of the polydicyclopentadiene, endowing it with excellent flame-retardant properties. Simultaneously, the reinforcing effect of the rigid aromatic rings on the side chains, combined with the hydrogen bonding effect of the polar groups, improves the material's heat resistance. Furthermore, the combined effect of the introduction of flexible segments of 1,5-dimethyl-1,5-cyclooctadiene and the rigid aromatic rings simultaneously enhances the toughness and strength of the polydicyclopentadiene. The resulting polydicyclopentadiene engineering material exhibits excellent flame-retardant properties and heat resistance, while also possessing a good balance of rigidity and toughness, meeting the application requirements of complex and harsh environments.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of polymer materials and engineering technology, specifically relating to a high heat-resistant, halogen-free intrinsically flame-retardant polydicyclopentadiene engineering material, and also to an intumescent norbornene-based flame retardant containing phenylphosphonic acyl and piperazine structures. Background Technology

[0002] Polydicyclopentadiene (PCD) is a high-performance thermosetting engineering material with high crosslinking density and numerous cyclic structural units in its main chain. Therefore, it maintains high modulus, high impact strength, and excellent solvent resistance in both high and low temperature environments, making it widely used in the automotive industry, large components of high-speed trains, and the medical field. However, as a fully carbon-chain polymer, PCD is highly flammable and prone to dripping during combustion, producing large amounts of smoke and toxic gases, limiting its application in complex environments. Although intumescent flame retardants exhibit good environmental friendliness due to their low smoke and halogen-free nature, the polarity difference between them and the matrix leads to uneven dispersion of the intumescent flame retardant within the matrix. While the composite material exhibits excellent flame retardancy, its mechanical properties are significantly reduced.

[0003] To address the aforementioned issues, domestic and international researchers have conducted extensive studies on improving the performance of polydicyclopentadiene. In patent CN 114835556A, researchers prepared a bromine-containing norbornene derivative and copolymerized it with dicyclopentadiene to prepare a flame-retardant polydicyclopentadiene composite material. The limiting oxygen index of this material reached 29%. However, halogen-containing flame retardants pose a significant environmental hazard, producing large amounts of smoke and releasing toxic gases. In patent CN 110183728A, researchers prepared an intumescent flame retardant and added it to polyolefins to prepare a flame-retardant polyolefin composite material. Although the flame retardant exhibited good flame retardancy, with a limiting oxygen index reaching 32.1%, the cantilever beam notched impact strength of the material was reduced. Therefore, in recent years, researchers have urgently sought to develop highly efficient, low-smoke, halogen-free, non-toxic flame retardants that can also improve the mechanical properties of materials.

[0004] This invention provides a class of intumescent norbornene-based flame retardants containing phenylphosphonic and piperazine structures. These flame retardants can be copolymerized with dicyclopentadiene and 1,5-dimethyl-1,5-cyclooctadiene monomers via thermally driven self-propagating technology. The resulting polydicyclopentadiene engineering material exhibits excellent flame retardant properties, heat resistance, and a good balance of rigidity and toughness. Its limiting oxygen index reaches 43%, its flame retardancy rating reaches UL-94V-0, its tensile strength reaches 131 MPa, its elongation at break reaches 48%, its impact strength reaches 108 kJ / m², and its heat distortion temperature reaches 199°C. Ultimately, a high-heat-resistant, halogen-free intrinsically flame-retardant polydicyclopentadiene engineering material is obtained. Summary of the Invention

[0005] One of the objectives of this invention is to provide a high-heat-resistant, halogen-free, intrinsically flame-retardant polydicyclopentadiene engineering material.

[0006] The second objective of this invention is to provide an intumescent norbornene-based flame retardant containing phenylphosphonic and piperazine structures, thereby solving the current problem of the flammability of polydicyclopentadiene and providing a novel intumescent intrinsic flame retardant with high flame retardant efficiency, low smoke, halogen-free, and non-toxic properties.

[0007] This invention further provides a preparation method in which the prepared intumescent norbornene-based flame retardant containing phenylphosphonic and piperazine structures can be copolymerized with dicyclopentadiene monomers via thermally driven self-propagating technology to finally obtain a high-heat-resistant, halogen-free intrinsically flame-retardant polydicyclopentadiene engineering material. This material has a limiting oxygen index of 43%, a flame retardancy rating of UL-94V-0, a tensile strength of 131 MPa, an elongation at break of 48%, an impact strength of 108 kJ / m², and a heat distortion temperature of 199°C. While possessing excellent flame retardant properties and heat resistance, it also exhibits a good balance of rigidity and toughness, meeting the application requirements of materials in complex and harsh environments.

[0008] The specific plan is as follows:

[0009] A high heat-resistant, halogen-free intrinsically flame-retardant polydicyclopentadiene engineering material, characterized in that the raw material comprises an intumescent norbornene-based flame retardant containing a phenylphosphonic acyl structure and a piperazine structure as shown in formula (1):

[0010]

[0011] In formula (1), R1 is an aliphatic or aromatic substituent with 0-6 carbon atoms, and R2 is an aliphatic or aromatic substituent with 0-6 carbon atoms.

[0012] The polydicyclopentadiene engineering material includes the structure shown in formula (2):

[0013]

[0014] In equation (2), m, n, and p are all independent integers between 50 and 800; R1 and R2 in equation (2) are the same as R1 and R2 in equation (1).

[0015] Furthermore, the present invention provides a method for preparing a high heat-resistant, halogen-free, intrinsically flame-retardant polydicyclopentadiene engineering material, wherein the total mass percentage of each raw material used to prepare the polydicyclopentadiene engineering material is 100 wt%, and the mass percentage of each raw material is as follows:

[0016] Dicyclopentadiene 49.65 wt%–69.80 wt%

[0017] 20wt%–40wt% of intumescent norbornene-based flame retardants containing phenylphosphonyl and piperazine structures

[0018] 1,5-Dimethyl-1,5-cyclooctadiene 10wt%

[0019] Ruthenium-based catalysts: 0.15 wt%–0.24 wt%

[0020] Inhibitor 0.05wt%~0.11wt%

[0021] The ruthenium-based catalyst is a second-generation Grubbs catalyst;

[0022] The inhibitor is a phosphate ester;

[0023] The preparation method of the high heat-resistant, halogen-free intrinsically flame-retardant polydicyclopentadiene engineering material includes:

[0024] (1) Disperse the expandable norbornene-based flame retardant containing phenylphosphonic and piperazine structures into a mixture containing dicyclopentadiene, 1,5-dimethyl-1,5-cyclooctadiene, Grubbs second-generation catalyst and inhibitor in proportion, and ultrasonically mix under ice-water bath conditions to obtain a dispersion.

[0025] (2) The dispersion is injected into the mold and local thermal initiation is carried out under heating conditions. Through its own thermal-driven self-propagating polymerization, the high heat-resistant halogen-free intrinsic flame-retardant polydicyclopentadiene engineering material is obtained by copolymerization.

[0026] Furthermore, the method also includes a method for synthesizing an intumescent norbornene-based flame retardant containing a phenylphosphonic acyl structure and a piperazine structure, comprising:

[0027] First, norbornene containing a monohydric alcohol and phenylphosphonic dichloride undergo a deHCl reaction in an organic solvent to obtain an intermediate containing a monohydric chloride. This reaction is carried out under the action of a catalyst at a temperature of 0-50℃ for 3-36 h. Then, this intermediate and a diol containing a piperazine structure undergo a deHCl reaction in an organic solvent. This reaction is carried out under the action of a catalyst at a temperature of 0-25℃ for 18-36 h, ultimately yielding the intumescent norbornene-based flame retardant containing both phenylphosphonic and piperazine structures.

[0028] Furthermore, in the method for synthesizing an intumescent norbornene-based flame retardant containing phenylphosphonic and piperazine structures, the catalyst required for the deHCl reaction is one or a mixture of several of the following: pyridine, sodium acetate, triethylamine, N,N-diisopropylethylamine, 4-pyrrolidinylpyridine, 4-N,N-dimethylpyridine, and 4-dimethylaminopyridine.

[0029] The organic solvent used in the deHCl reaction is at least one of the following: dichloromethane, trichloromethane, hexachloroethane, N,N-dimethylformamide, benzene, toluene, xylene, acetonitrile, and acetone.

[0030] Furthermore, the method for synthesizing the expandable norbornene-based flame retardant containing phenylphosphonic and piperazine structures includes:

[0031] First, the catalyst is added to a phenylphosphonic dichloride solution in a specific ratio. Then, norbornene containing a monohydric alcohol is added dropwise to the above mixed solution. Under nitrogen protection, the reaction is carried out at 0°C with stirring for 3-6 hours, and then at 25-50°C with stirring for 3-30 hours. After the reaction, the resulting mixture is washed, filtered, and dried. The product is then enriched to obtain an intermediate. Next, the intermediate, a dihydric alcohol containing a piperazine structure, and the catalyst are reacted under nitrogen protection at 0-25°C with stirring for 18-36 hours. After the reaction, the mixture is washed, filtered, and dried to obtain the intumescent norbornene-based flame retardant containing both phenylphosphonic and piperazine structures.

[0032] Furthermore, the molar ratio of the catalyst, phenylphosphonic dichloride, and norbornene containing a monohydric alcohol is 1:1.1:1.

[0033] Furthermore, the present invention provides an application of a high heat-resistant, halogen-free, intrinsically flame-retardant polydicyclopentadiene engineering material, which is used in bumpers, steering wheels, mudguard components for the automotive industry, high-temperature flame-retardant special protective clothing, and cable connector materials for high-speed trains.

[0034] The present invention has the following beneficial effects:

[0035] Compared with the prior art, the beneficial effects of the present invention are as follows:

[0036] (1) This invention provides a class of expandable norbornene-based flame retardant monomers containing phenylphosphonic and piperazine structures. During the combustion process of the composite material, the expandable flame retardant first produces phosphoric acid and pyrophosphate when heated. Then, under the catalysis of the piperazine group, it undergoes an esterification reaction with hydroxyl groups. The generated ester is dehydrated to form carbon, and the non-combustible gas generated at the same time causes the system to further expand and foam, forming an expanded porous carbon layer, which greatly improves the flame retardant performance of the material. This flame retardant monomer can be copolymerized with dicyclopentadiene monomer, and has the characteristics of high flame retardant efficiency, low smoke and halogen-free, and low toxicity. It is environmentally friendly and has no pollution to the environment. It is an ideal green and environmentally friendly flame retardant.

[0037] (2) This invention provides a class of expandable norbornene-based flame retardant monomers containing phenylphosphonic and piperazine structures. Rigid aromatic ring groups are introduced onto the side chains of polydicyclopentadiene molecules. The reinforcing effect of the rigid aromatic rings, combined with the hydrogen bonding effect of the polar groups, improves the heat resistance of the material. Furthermore, the combined effect of the introduction of flexible 1,5-dimethyl-1,5-cyclooctadiene segments and the rigid aromatic rings simultaneously improves the toughness and strength of polydicyclopentadiene.

[0038] (3) Compared with the traditional reaction injection molding curing process, the high heat-resistant halogen-free intrinsic flame-retardant polydicyclopentadiene engineering material of the present invention has a simple polymerization process and does not require secondary curing, and the industrialization process is simple. Attached Figure Description

[0039] Figure 1 The 1H-NMR spectrum of an expandable norbornene-based flame retardant A containing phenylphosphonyl and piperazine structures.

[0040] Figure 2 The 1H-NMR spectrum of an expandable norbornene-based flame retardant B containing phenylphosphonic and piperazine structures.

[0041] Figure 3 The 1H-NMR spectrum of norbornene-based flame retardant C containing a phenylphosphonyl structure.

[0042] Figure 4 1H-NMR spectrum of norbornene-based flame retardant D containing a piperazine structure

[0043] Figure 5 A flowchart illustrating the synthesis of an expandable norbornene-based flame retardant A containing phenylphosphonic and piperazine structures.

[0044] Figure 6 A flowchart illustrating the synthesis of an expandable norbornene-based flame retardant B containing phenylphosphonic and piperazine structures.

[0045] Figure 7 A flowchart illustrating the synthesis of norbornene-based flame retardant C containing a phenylphosphonic acyl structure.

[0046] Figure 8 A flowchart illustrating the synthesis of a norbornene-based flame retardant D containing a piperazine structure. Detailed Implementation

[0047] The present invention will be further described below with reference to specific embodiments. However, the scope of protection of the present invention is not limited to the following embodiments. Any non-essential adjustments and modifications made to the present invention based on the above description shall still fall within the scope of protection of the present invention.

[0048] The raw materials used in the following examples and comparative examples are:

[0049] Dicyclopentadiene, preferably from Sigma-Aldrich;

[0050] 1,5-Dimethyl-1,5-cyclooctadiene, preferably a product of Shanghai Aladdin Biochemical Technology Co., Ltd.;

[0051] Flame retardants A and B are intumescent norbornene-based flame retardants containing phenylphosphonic and piperazine structures, synthesized in this patent. Their structural formulas are detailed in Examples 1 and 6. Flame retardants C and D are norbornene-based flame retardants containing phenylphosphonic and piperazine structures, respectively, synthesized in this patent. Their structural formulas are detailed in Comparative Examples 5 and 6. The raw materials and catalysts include: 5-norbornene-2-methanol, 5-norbornene-2-ol, 5-norbornene-2-carboxylic acid, phenylphosphonic dichloro, N,N′-bis(2-hydroxyethyl)piperazine, 3-[4-(2-hydroxy-ethyl)-piperazin-1-yl]-1-propanol, triethylamine, dicyclohexylcarbodiimide, and 4-dimethylaminopyridine. Among them, 5-norbornen-2-methanol, 5-norbornen-2-ol, and 5-norbornen-2-carboxylic acid are preferably products of Sigma-Aldrich; phenylphosphonic dichloride is preferably a product of Shanghai Aladdin Biochemical Technology Co., Ltd.; N,N′-bis(2-hydroxyethyl)piperazine, 3-[4-(2-hydroxy-ethyl)-piperazin-1-yl]-1-propanol, triethylamine, dicyclohexylcarbodiimide, and 4-dimethylaminopyridine are preferably products of Shanghai Maclean Biochemical Technology Co., Ltd.; and the organic solvent used in the synthesis is preferably a product of Shanghai Aladdin Biochemical Technology Co., Ltd.

[0052] Flame retardant FRC-2 is an intumescent flame retardant, and products from Shanghai Aladdin Biochemical Technology Co., Ltd. are preferred.

[0053] Hexabromocyclododecane is a halogenated flame retardant, and antimony trioxide is an inorganic flame retardant aid. Products from Shanghai Maclean Biochemical Technology Co., Ltd. are preferred.

[0054] Grubbs' second-generation catalyst is a ruthenium-based catalyst, and the inhibitor is a phosphite, preferably a product from Sigma-Aldrich.

[0055] Table 1 lists the raw materials and quantities used in each embodiment.

[0056]

[0057]

[0058] To demonstrate the effectiveness of this invention, six comparative examples are provided:

[0059] Table 2 shows the raw materials and quantities used in each comparative example.

[0060]

[0061] Example 1

[0062] The high heat-resistant, halogen-free intrinsically flame-retardant polydicyclopentadiene engineering material of this embodiment comprises the following raw materials: 69.75 wt% dicyclopentadiene, 20 wt% flame retardant, 10 wt% 1,5-dimethyl-1,5-cyclooctadiene, 0.2 wt% Grubbs second-generation catalyst, and 0.05 wt% inhibitor. The flame retardant is an intumescent norbornene-based flame retardant A containing phenylphosphonyl and piperazine structures.

[0063] Its structural formula is:

[0064]

[0065] Flame retardant A (synthesis route diagram attached) Figure 5 Preparation of )

[0066] (1) First, 0.1 mol of triethylamine was added to a 150 mL three-necked flask containing 0.11 mol of phenylphosphonic dichloride in dichloromethane. The three-necked flask was connected to a condenser and a nitrogen inlet / outlet. Then, 0.1 mol of 5-norbornene-2-methanol was added dropwise to the above mixed solution. Under nitrogen protection, the mixture was stirred at 0 °C for 3 h, and then the temperature was gradually increased to 25 °C for 30 h. After the reaction was completed, the resulting mixture was extracted, washed, filtered, dried, and rotary evaporated. The product was then enriched to obtain the intermediate.

[0067] (2) Add 0.1 mol N,N′-bis(2-hydroxyethyl)piperazine, 0.09 mol of the intermediate obtained in step (1) and 0.1 mol 4-dimethylaminopyridine to a three-necked flask containing 150 mL of dichloromethane. The three-necked flask is connected to a condenser and a nitrogen inlet and outlet. Under nitrogen protection, the reaction is carried out at 25 °C with stirring for 18 h.

[0068] (3) After the reaction was completed, the resulting mixture was extracted, washed, filtered, dried and rotary evaporated multiple times. The organic phase was collected and subjected to rapid column chromatography with a mixture of dichloromethane and methanol as the eluent. The product was then enriched and characterized by 1H NMR to obtain an expandable norbornene-based flame retardant A containing phenylphosphonic amide structure and piperazine structure.

[0069] Preparation of high heat-resistant, halogen-free intrinsically flame-retardant polydicyclopentadiene engineering materials:

[0070] (1) 10 wt% 1,5-dimethyl-1,5-cyclooctadiene, 0.2 wt% Grubbs second-generation catalyst and 0.05 wt% inhibitor were added to 69.75 wt% dicyclopentadiene to obtain a mixture;

[0071] (2) Add 20wt% of the synthesized flame retardant A to the mixture and ultrasonically disperse the vial containing the mixture in an ice-water bath for 60s to obtain the dispersion.

[0072] (3) Finally, the dispersion is injected into a pre-made mold, and after local thermal initiation at 250°C, polymerization is carried out through its own heat-driven self-propagation. This yields the aforementioned high-heat-resistant, halogen-free, intrinsically flame-retardant polydicyclopentadiene engineering material.

[0073] Example 2

[0074] The high heat-resistant, halogen-free intrinsically flame-retardant polydicyclopentadiene engineering material of this embodiment comprises the following raw materials: 64.75 wt% dicyclopentadiene, 25 wt% flame retardant, 10 wt% 1,5-dimethyl-1,5-cyclooctadiene, 0.2 wt% Grubbs second-generation catalyst, and 0.05 wt% inhibitor. The flame retardant is an intumescent norbornene-based flame retardant A containing phenylphosphonyl and piperazine structures.

[0075] The preparation process of the flame-retardant polydicyclopentadiene engineering material in this embodiment is the same as in Embodiment 1.

[0076] Example 3

[0077] The high heat-resistant, halogen-free intrinsically flame-retardant polydicyclopentadiene engineering material of this embodiment comprises the following raw materials: 59.75 wt% dicyclopentadiene, 30 wt% flame retardant, 10 wt% 1,5-dimethyl-1,5-cyclooctadiene, 0.2 wt% Grubbs second-generation catalyst, and 0.05 wt% inhibitor. The flame retardant is an intumescent norbornene-based flame retardant A containing phenylphosphonyl and piperazine structures.

[0078] The preparation process of the flame-retardant polydicyclopentadiene engineering material in this embodiment is the same as in Embodiment 1.

[0079] Example 4

[0080] The high heat-resistant, halogen-free intrinsically flame-retardant polydicyclopentadiene engineering material of this embodiment comprises the following raw materials: 54.75 wt% dicyclopentadiene, 35 wt% flame retardant, 10 wt% 1,5-dimethyl-1,5-cyclooctadiene, 0.2 wt% Grubbs second-generation catalyst, and 0.05 wt% inhibitor. The flame retardant is an intumescent norbornene-based flame retardant A containing phenylphosphonyl and piperazine structures.

[0081] The preparation process of the flame-retardant polydicyclopentadiene engineering material in this embodiment is the same as in Embodiment 1.

[0082] Example 5

[0083] The high heat-resistant, halogen-free intrinsically flame-retardant polydicyclopentadiene engineering material of this embodiment comprises the following raw materials: 49.75 wt% dicyclopentadiene, 40 wt% flame retardant, 10 wt% 1,5-dimethyl-1,5-cyclooctadiene, 0.2 wt% Grubbs second-generation catalyst, and 0.05 wt% inhibitor. The flame retardant is an intumescent norbornene-based flame retardant A containing phenylphosphonyl and piperazine structures.

[0084] The preparation process of the flame-retardant polydicyclopentadiene engineering material in this embodiment is the same as in Embodiment 1.

[0085] Example 6

[0086] The high heat-resistant, halogen-free intrinsically flame-retardant polydicyclopentadiene engineering material of this embodiment comprises the following raw materials: 59.75 wt% dicyclopentadiene, 30 wt% flame retardant, 10 wt% 1,5-dimethyl-1,5-cyclooctadiene, 0.2 wt% Grubbs second-generation catalyst, and 0.05 wt% inhibitor. The flame retardant is an intumescent norbornene-based flame retardant B containing phenylphosphonic and piperazine structures.

[0087] Its structural formula is:

[0088]

[0089] Flame retardant B (synthesis route diagram attached) Figure 6 Preparation of )

[0090] (1) First, add 0.1 mol of triethylamine to a 150 mL three-necked flask containing 0.11 mol of phenylphosphonic dichloride in dichloromethane. Connect the three-necked flask to a condenser and a nitrogen inlet / outlet. Then, add 0.1 mol of 5-norbornen-2-ol dropwise to the above mixed solution. Under nitrogen protection, stir the mixture at 0 °C for 3 h, then gradually increase the temperature to 50 °C and continue the reaction for 3 h. After the reaction is complete, extract, wash, filter, dry, and rotary evaporate the resulting mixture, then enrich the product to obtain the intermediate.

[0091] (2) Add 0.1 mol of 3-[4-(2-hydroxy-ethyl)-piperazin-1-yl]-1-propanol, 0.09 mol of the intermediate prepared in step (1) and 0.1 mol of 4-dimethylaminopyridine to a three-necked flask containing 150 mL of dichloromethane. The three-necked flask is connected with a condenser and a nitrogen inlet and outlet. Under nitrogen protection, the reaction is carried out at 25 °C with stirring for 18 h.

[0092] (3) After the reaction was completed, the resulting mixture was extracted, washed, filtered, dried and rotary evaporated multiple times. The organic phase was collected and subjected to rapid column chromatography with a mixture of dichloromethane and methanol as the eluent. The product was then enriched and characterized by 1H NMR to obtain an expandable norbornene-based flame retardant B containing phenylphosphonic amide structure and piperazine structure.

[0093] The preparation process of the flame-retardant polydicyclopentadiene engineering material in this embodiment is the same as in Embodiment 1.

[0094] Example 7

[0095] The high heat-resistant, halogen-free intrinsically flame-retardant polydicyclopentadiene engineering material of this embodiment comprises the following raw materials: 59.75 wt% dicyclopentadiene, 30 wt% flame retardant, 10 wt% 1,5-dimethyl-1,5-cyclooctadiene, 0.2 wt% Grubbs second-generation catalyst, and 0.05 wt% inhibitor. The flame retardant is an intumescent norbornene-based flame retardant A and B containing phenylphosphonic and piperazine structures, in a ratio of 1:1.

[0096] The preparation process of the flame-retardant polydicyclopentadiene engineering material in this embodiment is the same as in Embodiment 1.

[0097] Comparative Example 1

[0098] The basic process and target structure in this comparative example are the same as in Example 1, but the preparation method is different. The specific preparation process is as follows:

[0099] (1) 0.1 mol N,N′-bis(2-hydroxyethyl)piperazine, 0.11 mol phenylphosphonic dichloride, and 0.1 mol 4-dimethylaminopyridine were added to a three-necked flask containing 150 mL of chloroform. The three-necked flask was connected to a condenser and a nitrogen inlet / outlet. Under nitrogen protection, the reaction was carried out at 30 °C with stirring for 2 h. After the reaction was completed, the resulting mixture was extracted and washed multiple times, dried, and the organic phase was collected to obtain the intermediate.

[0100] (2) Add 0.1 mol of 5-norbornene-2-methanol, 0.09 mol of the intermediate prepared in step (1) and 0.1 mol of triethylamine to a three-necked flask containing 150 mL of chloroform. The three-necked flask is connected to a condenser and a nitrogen inlet and outlet. Under nitrogen protection, the reaction is carried out at 40 °C with stirring for 18 h.

[0101] (3) After the reaction was completed, the resulting mixture was extracted, washed, filtered, dried and rotary evaporated multiple times. The organic phase was collected and subjected to rapid column chromatography with a mixture of chloroform and methanol as the eluent. The product was then enriched and characterized by 1H NMR. It was found that the target product could not be obtained.

[0102] Comparative Example 2

[0103] The flame-retardant polydicyclopentadiene engineering material of this comparative example includes the following raw materials: 99.75 wt% dicyclopentadiene, 0 wt% flame retardant, 0.2 wt% Grubbs II catalyst, and 0.05 wt% inhibitor.

[0104] The preparation process of the flame-retardant polydicyclopentadiene engineering material in this comparative example is the same as that in Example 1.

[0105] Comparative Example 3

[0106] The flame-retardant polydicyclopentadiene engineering material of this comparative example comprises the following raw materials: 59.75 wt% dicyclopentadiene, 30 wt% flame retardant, 10 wt% 1,5-dimethyl-1,5-cyclooctadiene, 0.2 wt% Grubbs second-generation catalyst, and 0.05 wt% inhibitor. The flame retardant is an additive intumescent flame retardant, FRC-2.

[0107] The preparation process of the flame-retardant polydicyclopentadiene engineering material in this comparative example is the same as that in Example 1.

[0108] Comparative Example 4

[0109] The flame-retardant polydicyclopentadiene engineering material of this comparative example comprises the following raw materials: 59.75 wt% dicyclopentadiene, 30 wt% flame retardant, 10 wt% 1,5-dimethyl-1,5-cyclooctadiene, 0.2 wt% Grubbs second-generation catalyst, and 0.05 wt% inhibitor. The flame retardant is a halogenated flame retardant, hexabromocyclododecane, and a synergist, antimony trioxide, in a ratio of 5:1.

[0110] The preparation process of the flame-retardant polydicyclopentadiene engineering material in this comparative example is the same as that in Example 1.

[0111] Comparative Example 5

[0112] The flame-retardant polydicyclopentadiene engineering material of this comparative example comprises the following raw materials: 59.75 wt% dicyclopentadiene, 30 wt% flame retardant, 10 wt% 1,5-dimethyl-1,5-cyclooctadiene, 0.2 wt% Grubbs second-generation catalyst, and 0.05 wt% inhibitor. The flame retardant is a norbornene-based flame retardant C containing a phenylphosphonic acyl structure.

[0113] Its structural formula is:

[0114]

[0115] Flame retardant C (synthesis route diagram attached) Figure 7 Preparation of )

[0116] First, 0.1 mol of 4-dimethylaminopyridine was added to a 150 mL dichloromethane mixture containing 0.11 mol of phenylphosphonyl dichloride. The flask was connected to a condenser and a nitrogen inlet / outlet. Then, 0.1 mol of 5-norbornene-2-methanol was added dropwise to the mixture. The reaction was carried out under nitrogen protection at 25 °C with stirring for 24 h. After the reaction was completed, the resulting mixture was subjected to multiple extractions, washing, filtration, drying, and rotary evaporation. The organic phase was collected and subjected to rapid column chromatography using a mixture of dichloromethane and methanol as the eluent. The product was then enriched and characterized by 1H NMR to obtain a norbornene-based flame retardant C containing a phenylphosphonyl structure.

[0117] The preparation process of the flame-retardant polydicyclopentadiene engineering material in this comparative example is the same as that in Example 1.

[0118] Comparative Example 6

[0119] The flame-retardant polydicyclopentadiene engineering material of this comparative example comprises the following raw materials: 59.75 wt% dicyclopentadiene, 30 wt% flame retardant, 10 wt% 1,5-dimethyl-1,5-cyclooctadiene, 0.2 wt% Grubbs second-generation catalyst, and 0.05 wt% inhibitor. The flame retardant is a norbornene-based flame retardant D containing a piperazine structure.

[0120] Its structural formula is:

[0121]

[0122] Flame retardant D (synthesis route diagram attached) Figure 8 Preparation of )

[0123] First, 0.1 mol of dicyclohexylcarbodiimide and 1 mmol of 4-dimethylaminopyridine were added to a 150 mL three-necked flask containing 0.11 mol of N,N′-bis(2-hydroxyethyl)piperazine in dichloromethane. The three-necked flask was connected to a condenser and a nitrogen inlet / outlet. Then, 0.1 mol of 5-norbornene-2-carboxylic acid was added dropwise to the above mixed solution. Under nitrogen protection, the mixture was stirred at 0 °C for 2 h, and then the temperature was gradually increased to 25 °C, and the reaction was continued for 5 h. After the reaction was completed, the resulting mixture was subjected to multiple extractions, washing, filtration, drying, and rotary evaporation. The organic phase was collected and subjected to rapid column chromatography using a mixture of dichloromethane and methanol as the eluent. The product was then enriched and characterized by 1H NMR to obtain a norbornene-based flame retardant D containing a piperazine structure.

[0124] The preparation process of the flame-retardant polydicyclopentadiene engineering material in this comparative example is the same as that in Example 1.

[0125] Tests and Results

[0126] The materials prepared in the above embodiments and comparative examples were cut to prepare test strips, and the testing method was as follows:

[0127] Enthalpy of polymerization and degree of cure: The enthalpy of polymerization and degree of cure were determined under a N2 atmosphere. For the enthalpy of polymerization test, the sample was first cooled to -10℃, held at that temperature for 5 min, and then heated to 200℃. The heating and cooling rates were 5℃ / min throughout the process. For the residual heat of reaction test, the sample was first heated to 250℃, held at that temperature for 5 min, then cooled to -20℃, and finally heated from -20℃ to 250℃. The heating and cooling rates were 10℃ / min throughout the process. The enthalpy of polymerization (Hr) and residual heat of reaction (Hres) were obtained, and the degree of cure α of the sample was calculated using the following formula:

[0128]

[0129] The molecular weight Mc between crosslinking points is calculated using the following formula:

[0130]

[0131] In the formula, ρ is taken as 1 g·cm⁻³, R is the ideal gas constant with a value of 8.314 J·mol⁻¹·K⁻¹, T is Tg+50 K, and E′Tg+50 K is the storage modulus of the sample at a temperature of Tg+50 K.

[0132] Tensile strength: Tested according to ISO 527-2:1993 standard at a speed of 50 mm / min.

[0133] Elongation at break: Tested according to ISO 527-2:1993 standard at a speed of 50 mm / min.

[0134] Impact resistance: Tested according to ISO 180:2000 standard.

[0135] Heat distortion temperature: tested according to ISO 75-2:2004 standard.

[0136] Limiting oxygen index: Tested according to GB / T 2406-1993 standard, sample size is 110mm×6mm×2mm.

[0137] UL-94: Tested according to GB / T 2048-1996 standard.

[0138] Cone calorimetry: Tested according to ISO 5660-1-2002 standard, the radiant power is 35kW / m2, and the sample size is 100mm×100mm×3mm.

[0139] Table 3. Polymerization kinetics, mechanical properties, heat resistance, and flame retardant properties of the high heat-resistant, halogen-free, intrinsically flame-retardant polydicyclopentadiene engineering materials prepared in Examples 1-7.

[0140]

[0141]

[0142] Table 4 shows the polymerization kinetics, mechanical properties, heat resistance, and flame retardant properties of the flame-retardant polydicyclopentadiene engineering materials prepared in Comparative Examples 1-6.

[0143]

[0144]

[0145] Tables 1 and 2 show the experimental formulations of Examples 1-7 and Comparative Examples 1-6, while Tables 3 and 4 show the polymerization kinetics, mechanical properties, heat resistance, and flame retardant properties of the flame-retardant polydicyclopentadiene engineering materials prepared in the corresponding Examples 1-7 and Comparative Examples 1-6.

[0146] The polymerization kinetics data for Examples 1-7 in Table 3 show that the introduction of comonomers reduced the heat of polymerization and degree of curing to some extent. This is because the steric hindrance effect caused by the introduction of flame-retardant units on the side chains of the expandable norbornene-based flame retardants containing phenylphosphonic and piperazine structures hindered the formation of the crosslinking network. Simultaneously, the introduction of the piperazine structure slightly reduced the activity of the Grubbs II catalyst. However, the degree of curing in all examples exceeded 97%, indicating that the materials still exhibited high curing properties. In Examples 1-7, with the increase of flame retardant content, the glass transition temperature of the polydicyclopentadiene engineering material increased from 160°C to a maximum of approximately 176°C, and the heat distortion temperature increased from 147°C to a maximum of 199°C, significantly improving the material's heat resistance. Characterization of the mechanical properties of the composite material revealed that the introduction of an intumescent norbornene-based flame retardant containing phenylphosphonic and piperazine structures significantly increased the tensile strength, elongation at break, and impact strength. This is because the combination of the introduction of the flexible 1,5-dimethyl-1,5-cyclooctadiene segment and the rigid aromatic ring simultaneously improved the toughness and strength of polydicyclopentadiene. Finally, characterization of the flame retardant properties of the composite material showed that the limiting oxygen index (LOI) increased from 18% to 43%, the peak heat release rate (pHRR) decreased by 86.27%, the burning growth rate (FIGRA) decreased by 96.16%, the peak smoke generation rate (pSPR) decreased by 81.03%, the fire performance index (FPI) increased by more than 12 times, the flame retardant rating reached UL-94V-0, and the char residue increased by 110.38%. The above results indicate that the introduction of intumescent norbornene-based flame retardants containing phenylphosphonic and piperazine structures greatly improves the char-forming ability and flame-retardant properties of polydicyclopentadiene composites.

[0147] Table 4 shows the relevant data results for Comparative Examples 1-6. In Comparative Examples 3-4, an additive intumescent flame retardant and a halogenated flame retardant were introduced into polydicyclopentadiene, respectively. The results showed that the additive intumescent flame retardant could only improve the flame retardant properties of the material, but the heat resistance and mechanical properties would decrease; the halogenated flame retardant, while improving the flame retardant properties, would produce a large amount of toxic fumes, causing environmental pollution. Furthermore, the flame retardant properties, heat resistance, and mechanical properties of the obtained polydicyclopentadiene material were significantly worse than those of the embodiments in this patent. In Comparative Examples 5-6, a self-synthesized norbornene-alkenyl flame retardant C containing a phenylphosphonic acid structure and a norbornene-alkenyl flame retardant D containing a piperazine structure were introduced into polydicyclopentadiene, respectively. The results showed that, compared with introducing the phenylphosphonic acid structure and the piperazine structure alone, the intumescent norbornene-alkenyl flame retardant containing both the phenylphosphonic acid structure and the piperazine structure could exert a synergistic flame retardant effect, resulting in better flame retardant performance.

[0148] In summary, the introduction of intumescent norbornene-based flame retardants containing phenylphosphonic and piperazine structures improves the flame retardancy and heat resistance of polydicyclopentadiene composites while maintaining a good balance of rigidity and toughness, thus meeting the application requirements of materials in complex and harsh environments.

[0149] Although the present invention has been described in detail through the above preferred embodiments, it should be understood that the above description should not be considered as a limitation of the present invention.

Claims

1. A method for producing a high heat-resistant halogen-free intrinsic flame-retardant polydicyclopentadiene engineering material, wherein the sum of the mass percentages of each raw material for producing the polydicyclopentadiene engineering material is 100 wt%, characterized in that, The mass percentages of each raw material are as follows: Dicyclopentadiene 49.65 wt%–69.80 wt% 20wt%–40wt% of intumescent norbornene-based flame retardants containing phenylphosphonyl and piperazine structures 1,5-Dimethyl-1,5-cyclooctadiene 10wt% Ruthenium-based catalysts: 0.15 wt%–0.24 wt% Inhibitor 0.05wt%~0.11wt% The ruthenium-based catalyst is a second-generation Grubbs catalyst; The inhibitor is a phosphate ester; The expanded norborneol-based flame retardant containing phenylphosphonic and piperazine structures has the structure shown in formula (1): ; In formula (1), R1 is an aliphatic or aromatic substituent with 0-6 carbon atoms, and R2 is an aliphatic or aromatic substituent with 0-6 carbon atoms. The preparation method of the high heat-resistant, halogen-free intrinsically flame-retardant polydicyclopentadiene engineering material includes: (1) Disperse the expandable norbornene-based flame retardant containing phenylphosphonic and piperazine structures into a mixture containing dicyclopentadiene, 1,5-dimethyl-1,5-cyclooctadiene, Grubbs second-generation catalyst and inhibitor in proportion, and ultrasonically mix under ice-water bath conditions to obtain a dispersion. (2) The dispersion is injected into the mold and local thermal initiation is carried out under heating conditions. Through its own thermal-driven self-propagating polymerization, the high heat-resistant halogen-free intrinsic flame-retardant polydicyclopentadiene engineering material is obtained by copolymerization.

2. The method according to claim 1, characterized in that: The method also includes a method for synthesizing an intumescent norbornene-based flame retardant containing phenylphosphonic and piperazine structures, comprising: First, norbornene containing a monohydric alcohol and phenylphosphonic dichloride undergo a deHCl reaction in an organic solvent to obtain an intermediate containing monochlorine. This reaction is carried out under the action of a catalyst at a temperature of 0-50℃ for 3-36 hours. Then, this intermediate and a diol containing a piperazine structure undergo a deHCl reaction in an organic solvent. This reaction is carried out under the action of a catalyst at a temperature of 0-25℃ for 18-36 hours, finally yielding the intumescent norbornene-based flame retardant containing phenylphosphonic and piperazine structures.

3. The method according to claim 2, characterized in that: The catalyst required for the deHCl reaction is one or a mixture of several of the following: pyridine, sodium acetate, triethylamine, N,N-diisopropylethylamine, 4-pyrrolidinylpyridine, and 4-dimethylaminopyridine. The organic solvent used in the deHCl reaction is at least one of the following: dichloromethane, trichloromethane, hexachloroethane, N,N-dimethylformamide, benzene, toluene, xylene, acetonitrile, and acetone.

4. The method according to claim 2 or 3, characterized in that: The method for synthesizing an expanded norborneol-based flame retardant containing phenylphosphonic and piperazine structures includes: First, the catalyst is added to a phenylphosphonic dichloride solution in a certain proportion to obtain a mixed solution. Then, norbornene containing a monohydric alcohol is added dropwise to the mixed solution. Under nitrogen protection, the reaction is carried out at 0°C with stirring for 3-6 hours, and then at 25-50°C with stirring for 3-30 hours. After the reaction is completed, the resulting reaction solution is washed, filtered, and dried. The product is then enriched to obtain an intermediate. The intermediate, a dihydric alcohol containing a piperazine structure, and the catalyst are then reacted under nitrogen protection at 0-25°C with stirring for 18-36 hours. After the reaction is completed, the product is washed, filtered, and dried to obtain the intumescent norbornene-based flame retardant containing phenylphosphonic and piperazine structures.

5. The method according to claim 2 or 3, characterized in that, In the deHCl reaction of norbornene containing a monohydric alcohol and phenylphosphonic dichloride in an organic solvent, the molar ratio of the catalyst, phenylphosphonic dichloride and norbornene containing a monohydric alcohol is 1:1.1:

1.

6. A high heat-resistant, halogen-free, intrinsically flame-retardant polydicyclopentadiene engineering material, said material being prepared by the method described in any one of claims 1-5.

7. Use of the highly heat resistant halogen-free intrinsically flame retardant polydicyclopentadiene engineering material according to claim 6, characterized in that: The high heat-resistant, halogen-free, intrinsically flame-retardant polydicyclopentadiene engineering material is used in automotive bumpers, steering wheels, mudguard components, high-temperature flame-retardant special protective clothing, and cable connectors for high-speed trains.

Citation Information

Patent Citations

  • In situ polymerization intumescent flame retardant and preparation raw materials as well as preparation method and application thereof

    CN110183728A

  • Bromine-containing norbornene derivative, preparation method thereof and flame-retardant polydicyclopentadiene material

    CN114835556A

  • High-modulus, high-impact, wear-resistant and heat-resistant intrinsic flame-retardant polydicyclopentadiene engineering material and preparation method thereof

    CN114790260A

  • Intrinsic flame-retardant polydicyclopentadiene elastomer material and preparation method thereof