A coal tar-based amorphous carbon and preparation method thereof
By introducing and controlling the role of bromine in the preparation process of amorphous carbon, a carbon network structure suitable for the insertion and deintercalation of lithium ions is formed, which solves the problem of underutilization of the effect of bromine on the performance of amorphous carbon and significantly improves the performance of amorphous carbon. electrochemical performance and stability.
Patent Information
- Application Number
- CN202111646891.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-12-29
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2041-12-29
AI Technical Summary
The effect of bromine on the structure and electrochemical performance of amorphous carbon is less common in the prior art, and there is a lack of detailed research, which limits the preparation method and performance improvement of amorphous carbon.
Low-temperature coal pitch is heated under a nitrogen atmosphere and liquid bromine is introduced. Coal pitch-based amorphous carbon is prepared through debromination polymerization and pre-carbonization. By controlling the introduction and removal of bromine, the directional formation is suitable for the insertion and deintercalation of lithium ions. The carbon network structure.
It increases the number of mesoporous structures and the orderliness of the carbon layer arrangement of amorphous carbon, significantly improves the reversible capacity and rate performance, and ensures the material's stability and high-temperature performance under high-current charge and discharge.
Smart Images

Figure BDA0003444084650000071 
Figure BDA0003444084650000082 
Figure BDA0003444084650000091
Abstract
Description
Technical Field
[0001] The present invention relates to the field of amorphous carbon preparation, and in particular to a coal-based amorphous carbon material and a preparation method thereof. Background Art
[0002] Unlike graphite, which has a perfect hexagonal crystal system, amorphous carbon refers to carbon materials with a low degree of graphitization and similar to an amorphous state. Depending on whether the precursor undergoes liquid phase carbonization or solid phase carbonization, amorphous carbon can be divided into soft carbon (graphitizable) and hard carbon (non-graphitizable). Soft carbon is composed of an organized region with a graphite-like structure and a highly twisted and cross-linked non-organized region. Typical soft carbons include mesophase carbon microspheres, petroleum coke, and needle coke; hard carbon belongs to non-graphitizable carbon, and its carbon network is generally a three-dimensional cross-linked structure. Common hard carbon materials include carbon black, resin-based carbon, and polymer pyrolytic carbon. Compared with graphite materials, amorphous carbon has a higher theoretical capacity (500-700mAh / g), better compatibility with electrolytes, and a higher diffusion coefficient of lithium ions in it, which helps the rapid embedding and de-embedding of lithium ions. In addition, the preparation of amorphous carbon does not require graphitization treatment, which has significant advantages in terms of cost. Therefore, as an important type of negative electrode material, amorphous carbon has been widely researched and developed.
[0003] Mochida used naphthalene and methylnaphthalene mesophase asphalt as precursors, pre-carbonized at 600°C for 30 minutes, then ground through a 325-mesh sieve, and calcined the sieved powder at 700-1200°C for 1 hour to obtain soft carbon. The authors analyzed the lithium storage mechanism of amorphous carbon and found that when the heat treatment temperature is higher than 800°C, the embedding of lithium ions is mainly achieved through intercalation; when the heat treatment temperature is lower than 800°C, the storage of lithium ions is mainly achieved through charge transfer of hexagonal plane mesh layers.
[0004] Fujimoto studied the effect of the introduction of oxygen on the structure and electrochemical properties of coal-tar-based hard carbon. Air or ammonium persulfate induced mild oxidation of the surface, and the pores formed were conducive to the insertion / deinsertion of lithium ions. However, phosphorus pentoxide had a strong oxidizing effect on the material, causing the pore structure to be destroyed and the amount of lithium insertion to be significantly reduced.
[0005] CN201711326231.1 proposes a method for preparing a hard carbon negative electrode material. Asphalt or resin is first mixed with an oxidant, and then subjected to low-temperature oxidation treatment (50-100°C), high-temperature oxidation treatment (110-250°C), pre-carbonization and carbonization treatment in sequence, to finally obtain a hard carbon material with high capacity and high first coulombic efficiency. The material has a first reversible capacity of 420mAh / g at 0.1C and a first coulombic efficiency of more than 81%.
[0006] CN201910384698.4 discloses a method for preparing an amorphous carbon material. The amorphous carbon material is prepared from a carbon-rich precursor through pretreatment, sintering, activation and hydrogenation reduction. Hydrogenation and deoxygenation effectively increase the lithium insertion sites, inhibit the occurrence of side reactions and battery flatulence, and improve the stability of the SEI film. The material exhibits excellent high-temperature performance (the capacity retention rate reaches 96% after 50 cycles at 60°C).
[0007] CN201711320084.7 reports a method for preparing a high-temperature resistant negative electrode material. The method uses soft carbon or hard carbon powder particles as the core, and sequentially coats carbon coating and nano coating from the inside to the outside. The nitrogen-containing or sulfur-containing multifunctional groups of the carbon coating effectively improve the wetting performance of the electrolyte on the amorphous carbon surface. The nano coating can react with HF generated during the charging and discharging process to protect the stabilized SEI film. The nano coating and functionalized carbon coating have a synergistic effect on the formation and stabilization of the SEI film at high temperature.
[0008] However, there are few reports on the effect of bromine on the structure and electrochemical properties of amorphous carbon. More studies are conducted on the effects of the introduction of oxygen, nitrogen and sulfur on the structure and electrochemical properties of amorphous carbon. If the role of bromine can be studied and explained in detail, it will be of great reference significance for expanding the preparation methods of amorphous carbon and improving the electrochemical properties of amorphous carbon. Summary of the invention
[0009] Therefore, the technical problem to be solved by the present invention is to provide a method for preparing amorphous carbon with excellent performance by using bromine.
[0010] The technical solution of the present invention is a method for preparing coal tar pitch-based amorphous carbon, comprising the following steps:
[0011] a. Low-temperature coal tar pitch is first heated to 120-150°C in a nitrogen atmosphere. Nitrogen purging is started before heating. Stirring is started after the tar is fully softened and in a fluid state. Liquid bromine is carried into the reaction system by nitrogen purging. The nitrogen blowing rate is 25-35 mL min -1 , the amount of bromine added is 5-30wt% of the low-temperature asphalt, and after the liquid bromine purge is completed, stirring and heat preservation are continued for 0.1-1h to obtain brominated coal tar pitch;
[0012] b. The brominated coal tar pitch is subjected to debromination polymerization reaction in a reaction vessel at a temperature of 350-420°C for 6-12 hours. From the early stage of the reaction to the stage of 200°C, the heating rate is 3-10°C / min; in the stage above 200°C, the heating rate is not higher than 2.5°C / min; the debromination product is ball-milled and sieved to obtain a powder solid 1; the powder solid 1 is pre-carbonized in a reaction vessel at a temperature of 550-700°C;
[0013] c. The pre-carbonized sample is ball-milled and then sieved to obtain a finer powder solid 2; the powder solid 2 is carbonized at 1000-1200° C. for 2-6 hours in an argon atmosphere in a reaction container to obtain coal-tar pitch-based amorphous carbon.
[0014] In step a, the bromine is not introduced in the form of droplets, but by passing nitrogen to purge the liquid bromine for reaction. For example, a three-necked flask is installed next to the main reactor, and the bromine is weighed and placed in the three-necked flask. This method can effectively disperse and reduce the concentration of bromine; the reason for introducing bromine in this way is mainly because the reaction activity of bromine is too high. If it is added in the form of droplets through a separatory funnel, it is easy to cause excessive local substitution reaction, resulting in uneven overall quality and even the risk of excessive cross-linking and coking. The introduction rate of liquid bromine is controlled by the nitrogen blowing rate and can be slowed down appropriately. The nitrogen blowing rate can be appropriately reduced in the later stage of the reaction. For example, the nitrogen blowing rate in the later stage of the reaction is 5-15mL·min -1 .
[0015] The late stage of the reaction not only includes the completion of the liquid bromine purge, but also includes a reaction stage before the completion of the liquid bromine purge. Since the introduction of bromine triggers a polymerization reaction, the viscosity of the system increases, and the diffusion of bromine becomes more difficult. Therefore, the amount of bromine introduced per unit time should be reduced. The disturbance of the liquid surface should be observed. If sufficient disturbance occurs, the stirring rate in the late stage should be much slower. During the entire reaction process, the preferred stirring rate is about 10-300rpm. More preferably, 20-200rpm. According to the viscosity of the liquid surface during the reaction process, the stirring rate is reduced when it is viscous, and the reaction rate is increased when it is thin.
[0016] In step b, the debromination reaction can be directly heated to debrominate; as for the heating rate, the heating rate can be appropriately increased in the early stage of the reaction (~200°C), and when the temperature is between 200-350°C or 200-420°C, the heating rate should not be too fast, generally not higher than 2.5°C / min, to ensure a relatively gentle debromination condensation reaction.
[0017] The atmosphere in step c is argon, which is more stable at high temperatures than nitrogen. Preferably, the gas velocity of argon is 100-200 mL·min -1 .
[0018] According to the method for preparing coal tar pitch-based amorphous carbon of the present invention, preferably, the low-temperature asphalt in step a is asphalt having a softening point of 60-70°C.
[0019] Preferably, the toluene soluble component TS content in the low-temperature asphalt is 85-95wt%; the toluene insoluble-pyridine soluble component TI-PS content is 5-9wt%; the pyridine insoluble-quinoline soluble component PI-QS content is 0.3-0.7wt%; and the quinoline insoluble component QI content is 0.5-3wt%.
[0020] Preferably, the heating method in step a is oil bath heating.
[0021] According to the method for preparing coal tar pitch-based amorphous carbon of the present invention, preferably, the reaction container in step b is a tubular furnace.
[0022] According to the method for preparing coal tar pitch-based amorphous carbon of the present invention, preferably, the sieving in step b is 40-100 mesh; and the sieving in step c is 300-400 mesh.
[0023] According to the method for preparing coal tar pitch-based amorphous carbon of the present invention, preferably, the pre-carbonization time in step b is 0.5-5h.
[0024] According to the method for preparing coal tar pitch-based amorphous carbon of the present invention, preferably, the heating rate in step c is 120-170° C. / h; and the insulation time after heating is 1-5 hours.
[0025] The present invention also provides a method for preparing coal tar pitch-based amorphous carbon, wherein the coal tar pitch-based amorphous carbon has a mesoporous structure of 2.0-4.5 nm; the coal tar pitch-based amorphous carbon has a discharge capacity of more than 280 mAh / g after 100 cycles at a current density of 200 mA g-1, and a capacity retention rate of more than 92%. The pore size distribution data can be referred to Figure 2 DFT pore size distribution; As for the ordered stacking and defect reduction, reference can be made to the TEM image of the amorphous carbon sample, which can support the increase in the degree of ordered stacking and the reduction in defects.
[0026] The invention discloses a method for preparing a coal-based amorphous carbon material, and specifically relates to the influence of bromine on the structure and electrochemical performance of coal-tar pitch-based amorphous carbon. The introduction of bromine increases the number of mesoporous structures, helps to increase the size of the amorphous carbon layer and improve the orderliness of the arrangement, and significantly improves the reversible capacity under high current charge and discharge.
[0027] The present invention uses low-temperature coal tar pitch (physical properties parameters see Table 1) with a softening point of about 65°C as raw material, and obtains coal tar pitch-based amorphous carbon through bromination, debromination polymerization, pre-carbonization and carbonization, and explains the effect of the introduction of bromine on the structure of amorphous carbon and its electrochemical properties.
[0028] Existing technologies generally involve direct carbonization of asphalt to prepare asphalt-based soft carbon, or a one-step oxidation / cross-linking reaction of asphalt (air oxidation, oxidant, cross-linking agent) to form a carbon-rich precursor with a three-dimensional cross-linked structure, which is then carbonized to obtain hard carbon with disordered stacking of carbon layers. Currently, there are no reports on the effect of bromine on the structure and properties of amorphous carbon.
[0029] The advantages of the present invention are:
[0030] 1. Different from conventional asphalt carbonization or oxidative carbonization, this process intends to modify and structurally induce the precursor asphalt by introducing and removing bromine, supplemented by fine control of the preparation process, to directionally control the formation of the carbon network and prepare amorphous carbon materials suitable for lithium ion embedding and de-embedding;
[0031] 2. The introduction of an appropriate amount of bromine helps the orderly stacking of the carbon layer and the reduction of defect sites, and the reversible capacity is improved;
[0032] 3. The introduction of bromine is conducive to the formation of mesoporous structure (2.0-4.5nm), which is convenient for the transmission of lithium ions and the infiltration of electrolyte, and the rate performance is improved;
[0033] 4. Bromine densifies amorphous carbon, improves carbon wall rigidity, and avoids the destruction of amorphous carbon structure under high current charge and discharge; BRIEF DESCRIPTION OF THE DRAWINGS
[0034] Figure 1 It is a flow chart of the present invention.
[0035] Figure 2 TEM image of an amorphous carbon sample.
[0036] Figure 3 DFT pore size distribution of amorphous carbon samples.
[0037] Figure 4 Rate performance curve of amorphous carbon sample.
[0038] Figure 5 It is the Raman spectrum of amorphous carbon sample. DETAILED DESCRIPTION
[0039] [Example 1]
[0040] Weigh 200 g of low-temperature coal tar pitch and put it into a 250 mL three-necked flask. Heat the oil bath to 120 °C. Turn on mechanical stirring (speed 75 rpm) and nitrogen purge (gas rate 30 mL min -1 ), after stirring for 0.5 h, weigh 30 g of liquid bromine and add it into a 100 mL three-necked flask. Connect the two three-necked flasks with a glass tube with rubber tubes at both ends. Reduce the nitrogen gas flow rate to 10 mL min -1 The bromination reaction was started. During the reaction, as the amount of bromine introduced increased, the viscosity of the system increased accordingly. The temperature was raised appropriately to ensure adequate stirring. After the liquid bromine was completely purged, the temperature was kept constant for 0.5 h to stop the reaction.
[0041] The brominated coal tar pitch was placed in a tubular furnace and heated to 410°C at a heating rate of 2°C / min and maintained for 10 hours under nitrogen atmosphere protection (gas rate). The debrominated asphalt was ground and pre-crushed and then placed in a planetary ball mill. The ball-milled sample was sieved through a 60-mesh sieve to obtain a powder solid sample.
[0042] The powder solid sample was placed in a horizontal tube furnace, heated to 600°C at a heating rate of 5°C / min and maintained for 0.5h. The obtained pre-carbonized sample was placed in a planetary ball mill, and the obtained ball-milled sample was sieved through a 325-mesh sieve to obtain a pre-carbonized powder sample.
[0043] The pre-carbonized powder sample was placed in a high-temperature box furnace and argon gas (gas rate 150 mL min -1 ), the temperature was raised to 1000°C at a heating rate of 150°C / h and maintained for two hours, and the obtained amorphous carbon sample was marked as AC15-1000.
[0044] [Example 2]
[0045] Weigh 200 g of low-temperature coal tar pitch and put it into a 250 mL three-necked flask. Heat the oil bath to 120 °C. Turn on mechanical stirring (speed 75 rpm) and nitrogen purge (gas rate 30 mL min -1 ), after stirring for 0.5 h, weigh 60 g of liquid bromine and add it into a 100 mL three-necked flask. Connect the two three-necked flasks with a glass tube with rubber tubes at both ends. Reduce the nitrogen gas flow rate to 10 mL min -1 The bromination reaction was started. During the reaction, as the amount of bromine introduced increased, the viscosity of the system increased accordingly. The temperature was raised appropriately to ensure adequate stirring. After the liquid bromine was completely purged, the temperature was kept constant for 0.5 h to stop the reaction.
[0046] The brominated coal tar pitch was placed in a tubular furnace and heated to 410°C at a heating rate of 2°C / min and maintained for 10 hours under nitrogen atmosphere protection (gas rate). The debrominated asphalt was ground and pre-crushed and then placed in a planetary ball mill. The ball-milled sample was sieved through a 60-mesh sieve to obtain a powder solid sample.
[0047] The powder solid sample was placed in a horizontal tube furnace, heated to 600°C at a heating rate of 5°C / min and maintained for 0.5h. The obtained pre-carbonized sample was placed in a planetary ball mill, and the obtained ball-milled sample was sieved through a 325-mesh sieve to obtain a pre-carbonized powder sample.
[0048] The pre-carbonized powder sample was placed in a high-temperature box furnace and argon gas (gas rate 150 mL min -1 ), the temperature was raised to 1000°C at a heating rate of 150°C / h and maintained for two hours, and the obtained amorphous carbon sample was marked as AC30-1000.
[0049] [Example 3]
[0050] Weigh 200 g of low-temperature coal tar pitch and put it into a 250 mL three-necked flask. Heat the oil bath to 120 °C. Turn on mechanical stirring (speed 75 rpm) and nitrogen purge (gas rate 30 mL min -1 ), after stirring for 0.5 h, weigh 30 g of liquid bromine and add it into a 100 mL three-necked flask. Connect the two three-necked flasks with a glass tube with rubber tubes at both ends. Reduce the nitrogen gas flow rate to 10 mL min -1 The bromination reaction was started. During the reaction, as the amount of bromine introduced increased, the viscosity of the system increased accordingly. The temperature was raised appropriately to ensure adequate stirring. After the liquid bromine was completely purged, the temperature was kept constant for 0.5 h to stop the reaction.
[0051] The brominated coal tar pitch was placed in a tubular furnace and heated to 410°C at a heating rate of 2°C / min and maintained for 10 hours under nitrogen atmosphere protection (gas rate). The debrominated asphalt was ground and pre-crushed and then placed in a planetary ball mill. The ball-milled sample was sieved through a 60-mesh sieve to obtain a powder solid sample.
[0052] The powder solid sample was placed in a horizontal tube furnace, heated to 600°C at a heating rate of 5°C / min and maintained for 0.5h. The obtained pre-carbonized sample was placed in a planetary ball mill, and the obtained ball-milled sample was sieved through a 325-mesh sieve to obtain a pre-carbonized powder sample.
[0053] The pre-carbonized powder sample was placed in a high-temperature box furnace and argon gas (gas rate 150 mL min -1 ), the temperature was raised to 1200 °C at a heating rate of 150 °C / h and maintained for 2 h. The obtained amorphous carbon sample was labeled AC15-1200.
[0054] [Comparative Example 1]
[0055] Weigh 200 g of low-temperature coal tar pitch and put it into a 250 mL three-necked flask. Heat the oil bath to 120 °C. Turn on mechanical stirring (speed 75 rpm) and nitrogen purge (gas rate 30 mL min -1 ), and stop the reaction after keeping warm for 2 h.
[0056] The above sample was placed in a tubular furnace and heated to 410°C at a heating rate of 2°C / min and maintained for 10 hours under nitrogen atmosphere protection (gas rate). The debrominated asphalt was ground and pre-crushed and then placed in a planetary ball mill. The ball-milled sample was sieved through a 60-mesh sieve to obtain a powder solid sample.
[0057] The powder solid sample was placed in a horizontal tube furnace, heated to 600°C at a heating rate of 5°C / min and maintained for 0.5h. The obtained pre-carbonized sample was placed in a planetary ball mill, and the obtained ball-milled sample was sieved through a 325-mesh sieve to obtain a pre-carbonized powder sample.
[0058] The pre-carbonized powder sample was placed in a high-temperature box furnace and argon gas (gas rate 150 mL min -1 ), the temperature was raised to 1000 °C at a heating rate of 150 °C / h and maintained for 2 h. The obtained amorphous carbon sample was marked as AC0-1000.
[0059] Half-cell assembly and testing methods:
[0060] Amorphous carbon material, Super C and polyvinylidene fluoride were uniformly dispersed in N-methyl-2-pyrrolidone at a mass ratio of 8:1:1, the slurry was uniformly coated on the copper foil current collector and vacuum dried at 110°C; then a CR2016 button half-cell was assembled in a glove box, with a lithium sheet as the counter electrode, Celgard 2400 as the separator, and the electrolyte was 1mol / LLiPF6 / EC+DMC+EMC (volume ratio 1:1:1). Constant current charge and discharge tests were performed on a LAND CT2001A instrument with a charge and discharge voltage range of 0-2V.
[0061] Table 1 General physical properties of coal tar pitch raw materials
[0062]
[0063]
[0064] a ΔDiff.=100-CHN.
[0065] Compared with AC0-1000, the introduction of bromine improves the orientation of carbon layer arrangement of amorphous carbon samples on the one hand. The regular carbon layer orientation is conducive to the transmission of lithium ions and the improvement of reversible capacity; on the other hand, bromine helps to increase the molecular weight and degree of polymerization of coal tar, the size of amorphous carbon crystallites increases, and the number of lithium storage sites between graphite sheets increases.
[0066] Table 2 Pore structure parameters of amorphous carbon
[0067]
[0068] Compared with AC0-1000, the introduction of bromine significantly increases the number of mesoporous structures (2.0-4.5 nm). The presence of these mesoporous structures is conducive to the full infiltration of the electrolyte and the amorphous carbon material and the transmission of lithium ions therein, thereby improving the rate performance.
[0069] Compared with AC0-1000, the introduction of bromine significantly increased the discharge capacity of the amorphous carbon sample at various current densities. The capacity difference was more obvious at high current density. -1 Back to 50mA g -1When the initial capacity of AC15-1000 and AC30-1000 was restored, AC0-1000 only restored to 86% of the initial capacity, which indicates that the introduction of bromine helps to maintain the amorphous carbon structure. Figure 2-Figure 5 .
[0070] In order to illustrate the reduction of defect sites, Raman spectroscopy analysis was carried out on the samples. The results showed that the ID / IG values of AC0-1000, AC15-1000 and AC30-1000 were 1.05, 0.99 and 1.01, respectively, indicating that the introduction of bromine is helpful to the reduction of defect sites and the orderly stacking of graphite sheets, which is consistent with the TEM results.
[0071] As for the reversible capacity, the cycle performance of samples AC0-1000 and AC15-1000 at a current density of 200mA g-1 are as follows: after 100 cycles, the discharge capacity of AC15-1000 is 286mAh / g, and the capacity retention rate is 92.9%; after 100 cycles, the discharge capacity of AC0-1000 is 274mAh / g, and the capacity retention rate is 90.1%. It can be seen that the cycle performance of AC15-1000 is better than that of AC0-1000, and the introduction of bromine is conducive to the improvement of the material's cycle performance, which is due to a certain number of mesoporous structures in AC15-1000 and the sufficient infiltration of the electrolyte and the material.
[0072] Figure 4 The rate performance curve shows that the introduction of appropriate bromine can significantly improve the rate performance.
[0073] Table 3 Capacity of coal-based amorphous carbon at different current densities with different bromine introduction amounts as a percentage of the capacity at 50 mA g-1
[0074]
[0075] 100mA g -1 The capacity retention rates of the samples were similar when the current density was higher than 200 mA g -1 When the rate capacity retention of each sample is 20%, the rate capacity retention rate of each sample is significantly different. Among them, AC15-1000 has the highest rate capacity retention rate, followed by AC30-1000, and AC0-1000 has the lowest rate capacity retention rate. This is mainly because the debrominated asphalt-based amorphous carbon contains a considerable number of mesoporous structures, which is conducive to the Li + When the current density drops back to 50 mA g -1When charged and discharged at high currents, the capacity of AC0-1000 is only 86% of the initial capacity, which is lower than that of AC15-1000 (97.7%) and AC30-1000 (96.0%). This may be due to the change in the material structure under high current charge and discharge, which leads to a decrease in the amount of lithium embedded.
Claims
1. A method for preparing coal tar pitch-based amorphous carbon, characterized in that: The steps include: a. The low-temperature coal tar pitch is first heated to 120-150°C in a nitrogen atmosphere, and nitrogen purging is started before heating. Stirring is started after the mixture is fully softened and in a fluid state. Liquid bromine is carried into the reaction system by nitrogen purging. The nitrogen blowing rate is 25-35 mL / min, and the amount of bromine added is 5-30 wt% of the low-temperature coal tar pitch. After the liquid bromine purging is completed, stirring and heat preservation are continued for 0.1-1h to obtain brominated coal tar pitch; the low-temperature coal tar pitch is an asphalt with a softening point of 60-70°C; the content of toluene-soluble components TS in the low-temperature coal tar pitch is 85-95wt%; the content of toluene-insoluble-pyridine-soluble components TI-PS is 5-9wt%; the content of pyridine-insoluble-quinoline-soluble components PI- QS is 0.3-0.7wt%; the content of quinoline-insoluble components QI is 0.5-3wt%; b. The brominated coal tar pitch is subjected to debromination polymerization reaction in a reaction vessel at a temperature of 350-420°C for 6-12 h. From the early stage of the reaction to the stage of 200°C, the heating rate is 3-10°C / min; in the stage above 200°C, the heating rate is not higher than 2.5°C / min; the debromination product is ball-milled and sieved to obtain a powder solid 1; the powder solid 1 is pre-carbonized in a reaction vessel at a temperature of 550-700°C; c. The pre-carbonized sample is ball-milled and then sieved to obtain a finer powder solid 2; the powder solid 2 is carbonized at 1000-1200°C for 2-6 hours in an argon atmosphere in a reaction container to obtain coal tar pitch-based amorphous carbon; the coal tar pitch-based amorphous carbon has a mesoporous structure of 2.0-4.5 nm; the coal tar pitch-based amorphous carbon has a discharge capacity of more than 280 mAh / g after 100 cycles at a current density of 200 mA g-1, and a capacity retention rate of more than 92%.
2. The method for preparing a coal tar pitch-based amorphous carbon according to claim 1, characterized in that: The reaction vessel in step b is a tubular furnace.
3. The method for preparing a coal tar pitch-based amorphous carbon according to claim 1, characterized in that: The mesh size of the sieve in step b is 40-100 meshes.
4. The method for preparing a coal tar pitch-based amorphous carbon according to claim 1, characterized in that: The sieve in step c is 300-400 mesh.
5. The method for preparing a coal tar pitch-based amorphous carbon according to claim 1, characterized in that: The pre-carbonization time in step b is 0.5-5h.
6. The method for preparing a coal tar pitch-based amorphous carbon according to claim 1, characterized in that: In step c, in an argon atmosphere, the temperature is raised to 1000-1200° C. at a rate of 120-170° C. / h and carbonized for 2-6 hours to obtain coal-tar pitch-based amorphous carbon.