A hydrogenation method for producing food grade white oil

By using pre-refined distillate oil or hydrocracking tail oil in the white oil hydrogenation reaction to carry out the hydroisomerization reaction, and using an amorphous silicon-aluminum-based highly dispersed platinum and palladium catalyst, the problem of food-grade white oil in the existing technology is solved. Oil production problems have been solved, and food-grade white oil that meets national standards has been efficiently produced, improving the viscosity and stability of the product.

CN116410783BActive Publication Date: 2024-10-15PETROCHINA CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111671611.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-12-31
Publication Date
2024-10-15
Estimated Expiration
2041-12-31

AI Technical Summary

Technical Problem

It is difficult to effectively produce high-purity food-grade white oil with existing technology, especially in improving the depth of aromatic hydrocarbon removal and controlling reaction conditions. This has led to a shortage of high-viscosity food-grade white oil in the domestic market.

Method used

Pre-refined distillate or hydrocracking tail oil is used for hydroisomerization reaction, and an amorphous silica-aluminum-based highly dispersed platinum-palladium white oil hydrogenation catalyst is used to perform olefin saturation in a fixed-bed white oil hydrogenation reactor. , aromatic hydrocarbon saturation reaction to prepare products that meet food-grade white oil standards. The catalyst improves the activity and dispersion of the catalyst by preparing a composite buffer solution, modifying the silicon-aluminum carrier and loading platinum and palladium.

Benefits of technology

The production of low, medium and high viscosity food-grade white oil has been realized. The UV absorbance of condensed ring aromatic hydrocarbons of the product meets the national standards, and the oxidation stability and photothermal stability are excellent. It meets the No. 1-4 food-grade white oil standards and improves the quality of white oil. Oil production efficiency and quality.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116410783B_ABST
    Figure CN116410783B_ABST
Patent Text Reader

Abstract

The present invention discloses a hydrogenation method for producing food-grade white oil, wherein a pre-refined vacuum distillate oil or a hydrocracking tail oil is subjected to a hydrogenation isomerization reaction to obtain an isomerized product oil, and the isomerized product oil is introduced into a fixed-bed white oil hydrogenation reactor, wherein the isomerized product oil undergoes olefin saturation and aromatic saturation reactions, and is characterized in that a white oil hydrogenation catalyst is added to the fixed-bed white oil hydrogenation reactor, and the catalyst is an amorphous silicon-aluminum-based highly dispersed platinum-palladium white oil hydrogenation catalyst. The food-grade white oil obtained by the present invention has a water-white appearance, excellent oxidation stability and photothermal stability. The polycyclic aromatics ultraviolet absorbance of the product is ≯0.1cm, the color is +30, and the easy carbide passes, and other indicators meet the national standard GB / 1886.215-2016 for food-grade white oil No. 1-4.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a hydrogenation method for producing food-grade white oil. Background Art

[0002] As a high-value-added specialty product of oil refining, the domestic consumption of white oil has exceeded 2 million tons / year, among which the added value of high-purity food-grade and pharmaceutical-grade white oil is much greater than that of industrial-grade white oil. With the development of the food and pharmaceutical industries and the need for health and safety in China, the demand for high-grade food and pharmaceutical-grade white oil has increased year by year, accounting for more than 20% of the total demand. Since the processing of food and pharmaceutical-grade white oil requires higher hydrogenation technology and strict indicators, domestic enterprises are still restricted in production, and there is still a shortage of high-viscosity food-grade white oil in the domestic market. According to statistics in 2019, in order to meet market needs, the addition of high-end white oil devices in China is on the agenda. At present, domestic production enterprises are working hard to reverse the situation of high-end white oil dependence on imports, and market practitioners are seeking high-end white oil products that can replace imports, which is conducive to the promotion of the domestic high-end white oil market.

[0003] The most difficult thing to remove in the deep hydrogenation reaction of white oil is polycyclic aromatic hydrocarbons, which requires not only that the catalyst has an open pore structure to eliminate its diffusion effect, but also that it has a suitable acid distribution to adsorb aromatic hydrocarbons. Therefore, the development of a carrier with an open pore structure and suitable acid properties has become a key issue in the development of high-performance white oil hydrogenation catalysts.

[0004] Chinese patent CN101747937B discloses a method for preparing food-grade naphthenic white oil using a noble metal aromatic saturation catalyst. The amorphous silicon-alumina carrier has a specific surface area of ​​300 cm 2 ·g -1 , pore volume 0.9 cm 3 ·g -1 , average pore size 5-15nm. The total platinum-palladium loading of the catalyst exceeds 1wt%, the reaction pressure is not more than 20MPa, the reaction temperature is 180ˉ300℃, the hydrogen-oil volume ratio is 1000:1, and the space velocity is 1.0h -1 Under the conditions of , the naphthenic base oil was used as the raw material to produce white oil products that meet the GB / T4853-94 food grade white oil standard. However, the reaction conditions are harsh and the cost is high.

[0005] Chinese patent CN106753550A discloses a method for producing food-grade white oil by hydrogenating naphthenic lubricating base oil, wherein noble metal catalysts with different acidity are graded, the catalyst in the second catalyst bed is more acidic than the catalyst in the first catalyst bed, and the reactor is zoned to control the reaction temperature. However, the temperature of the first bed is 40-50℃ higher than that of the second bed, which places higher requirements on the reaction device.

[0006] Chinese patent CN109266388A discloses a white oil hydrogenation production method based on a composite catalyst. The composite catalyst uses polymer microspheres as a template, which are calcined to form a hollow structure inside and porous structure outside. Stearic acid is used to modify the alumina microspheres to increase the number and dispersion of active centers. The composite catalyst is used to perform deep hydrogenation of hydrocracking tail oil at a reaction pressure of 10MPa, a reaction temperature of 310℃, a hydrogen-to-oil volume ratio of 650:1, and an air velocity of 1.1h -1 Under these conditions, high-quality industrial white oil can be produced, but food-grade white oil cannot be produced.

[0007] White oil is a special oil product that has been refined to a very high degree. It belongs to the lubricating oil fraction. It is colorless, tasteless, odorless, chemically inert, and has excellent light and thermal stability. It has a wide range of uses. As an emerging petroleum product, white oil is being valued by the domestic refining industry. The classification of white oil is generally divided into two categories abroad: one is industrial grade white oil, and the other is food and pharmaceutical grade white oil. In my country, white oil is divided into three grades: industrial grade, cosmetic grade, and food and pharmaceutical grade. Its main property indicators are: viscosity difference, color, easy carbonization, ultraviolet absorption, freezing point, etc. The application of food and pharmaceutical grade white oil requires that the oil must be non-toxic and harmless, with a low pour point, high flash point and boiling point, low volatility, non-corrosive, and have good oxidation stability and thermal stability. my country's national standard for food-grade white oil GB / 1886.215-2016 stipulates that the ultraviolet absorbance of polycyclic aromatic hydrocarbons in food-grade white oil is ≯0.1cm and the color is +30.

[0008] Due to the high degree of refining required for medium and high-grade white oil, the medium and high viscosity grades of white oil currently produced in my country cannot cover the full viscosity range, and some varieties still need to be imported. White oil has different grades and specifications, and its price varies greatly, often several times or even dozens of times. Generally, the higher the viscosity of the white oil product, the higher the price and the higher the profit. At present, the domestic white oil market in my country is unevenly developed, mainly producing industrial-grade white oil. The annual production capacity of food-grade, cosmetic-grade, and pharmaceutical-grade white oil accounts for about 16% of the total domestic production capacity, of which the food-grade white oil production capacity accounts for about 5%. Only a small number of refineries in China produce food-grade white oil. In 2019, the domestic refineries that meet the standards for producing food-grade white oil include Daqing Refining and Chemical, Karamay Petrochemical, Tianjin Kaiwei Yongli, Shandong Qingyuan Petrochemical, and Shandong Yellow River New Materials, with a total production capacity of 360,000 tons / year.

[0009] With the steady growth of my country's economic situation, the demand for white oil is increasing, and the quality requirements for white oil are also increasing. Therefore, the research and production of food-grade white oil is of great significance. In the field of white oil hydrogenation catalyst research, my country has developed a series of high-activity white oil hydrogenation catalysts: "NJBMDA series catalysts" of Nanjing Bo Ming Technology Co., Ltd., "C-LUBE series catalysts" of CRITERION, "3872 (RA-1) catalyst", "RDA-II catalyst", "RLF-10 w Catalyst", "RLF-20 catalyst", "HPO-1 catalyst" developed by Changchun Huigong Catalyst Co., Ltd., etc.

[0010] At present, the production of food-grade white oil mainly adopts the two-stage hydrogenation process. The white oil raw material is firstly treated with a non-precious metal catalyst to remove the sulfur and nitrogen components, and at the same time saturate most of the aromatics. Then the remaining aromatics are deeply removed by a second stage of precious metal catalyst, and the light fraction is removed by fractionation to obtain the white oil product. The two-stage hydrogenation process can process a variety of white oil raw materials to produce different types of white oil products. At present, food and medical grade white oil products are all produced by multi-stage hydrogenation processes. The pressure of the two-stage hydrogenation process can reach 22MPa, and the air velocity generally does not exceed 1.0h -1 The reaction conditions are already very harsh. To further improve the depth of aromatic removal, a high-activity catalyst is the key. Summary of the invention

[0011] The object of the present invention is to provide a new hydrogenation method for producing food-grade white oil, which is particularly suitable for producing low, medium and high viscosity food-grade white oil by using pre-refined distillate oil or hydrocracking tail oil.

[0012] As one aspect of the present invention, it relates to a hydrogenation method for producing food-grade white oil. Pre-refined vacuum distillate oil or hydrocracking tail oil is subjected to a hydrogenation isomerization reaction to obtain isomerized product oil. The isomerized product oil enters a fixed-bed white oil hydrogenation reactor. The isomerized product oil undergoes olefin saturation and aromatic saturation reactions. A white oil hydrogenation catalyst is added to the fixed-bed white oil hydrogenation reactor. The catalyst is an amorphous silicon-aluminum-based highly dispersed platinum-palladium white oil hydrogenation catalyst.

[0013] In at least one specific embodiment, the amorphous silicon-aluminum-based highly dispersed platinum-palladium white oil hydrogenation catalyst is prepared as follows:

[0014] 1. Preparation of carrier:

[0015] (1) Preparation of composite buffer solution: Prepare a solution using triethanolamine, deionized water and ammonium dihydrogen phosphate.

[0016] (2) Add the silicon source and aluminum source dropwise into the buffer solution to maintain a stable pH for precipitation.

[0017] (3) The solution obtained in step (2) is crystallized, washed, dried and calcined.

[0018] The triethanolamine buffer solution in the present invention plays the following roles in the synthesis system: 1. adjusting the pH value to keep the whole system stable and reduce the fluctuation of product quality; 2. triethanolamine can react with Al(OH)4 - Complexation to form Al(OH)(OCH2CH2)3N - , enhance the dissolution of aluminum source, and release Al(OH)4 at high temperature crystallization - Cross-link with silicon source; ③ Phosphoric acid can improve the acidity of amorphous silicon-aluminum materials and increase their acidic sites.

[0019] 2. Loading of active metals:

[0020] (4) Modification of amorphous silica-alumina support with urea

[0021] The amorphous silica-alumina carrier was mixed with urea and ground into 320 mesh, and then calcined in a covered crucible. The temperature was first increased to 150°C at a rate of 1°C / min for 2 h, and then increased to 300°C at a rate of 1°C / min for 2 h, and then washed with water and alcohol three times.

[0022] (5) Platinum-palladium active metals are loaded onto the previously prepared support by an equal volume impregnation method, and then dried and calcined to obtain a highly dispersed platinum-palladium white oil hydrogenation catalyst.

[0023] In at least one specific embodiment, in step (4), the mass ratio of amorphous silicon aluminum to urea is 0.45-0.55. The calcination temperature is 150° C. for 2 h, and 300° C. for 2 h.

[0024] In at least one specific embodiment, in the step (5), Pt is derived from any one of tetraammineplatinum nitrate, platinum acetate, platinum nitrate and chloroplatinic acid, and Pd is derived from any one of tetraamminepalladium nitrate, palladium nitrate, chloropalladic acid, palladium chloride and dichlorodiamminepalladium.

[0025] In at least one specific embodiment, the active metal content in step (5) is Pt 0.4 wt%, Pd 0.2 wt%.

[0026] In at least one specific embodiment, in step (1), the pH of the buffer solution is 11-12.

[0027] In at least one specific embodiment, the reaction conditions in step (2) are a temperature of 70° C. and a stable pH of 11.3-11.8.

[0028] In at least one specific embodiment, the crystallization conditions in step (3) include: a temperature of 140° C. and a time of 24 hours, thereby improving the performance of the obtained amorphous silicon aluminum and significantly improving the catalytic activity of the catalyst.

[0029] In at least one specific embodiment, in step (2), the silicon source is preferably an acidic silica sol with a particle size of 10 nm.

[0030] In at least one specific embodiment, in step (2), the aluminum source is preferably aluminum sulfate.

[0031] In at least one specific embodiment, the buffer solution is prepared by mixing triethanolamine, deionized water and ammonium dihydrogen phosphate in a mass ratio of 5:50:2, the silicon source is a silica sol with a particle size of 10 nm, and the aluminum source is aluminum sulfate. Aluminum sulfate is prepared into a 1 mol / L solution and added to the buffer solution while stirring. After the addition is completed, stirring is continued for 20 minutes. The silica sol is diluted with deionized water and slowly added dropwise to the buffer solution while stirring. After the addition is completed, stirring is continued for 30 minutes. The amount of buffer solution should be able to maintain the pH stable at 11.3-11.8 during the addition of the silica-alumina solution. The obtained mixed solution is then added to the crystallization kettle and crystallized at 140°C for 24 hours.

[0032] In at least one specific embodiment, in step (2), the amount of the acidic silica sol and aluminum sulfate is calculated based on the mass fraction of SiO2 and Al2O3, and the mass fraction of SiO2 accounts for 50%, thereby improving the acidity of amorphous silica aluminum and significantly improving the catalytic activity of the catalyst.

[0033] In at least one specific embodiment, in step (3), the method may further include: adding aluminum sulfate and silica sol in parallel to the buffer solution obtained in step (1) under stirring conditions, and the stirring speed may be 600 r / min.

[0034] In at least one specific embodiment, in step (3), the drying conditions may be various drying conditions in the art, for example, may include: temperature of 60° C. and time of 24 h.

[0035] In at least one specific embodiment, in step (3), the calcination conditions may be various calcination conditions in the art, for example, the calcination temperature is 500° C. and the calcination time is 3 h.

[0036] The water used in the present invention can be at least one of pure water, distilled water and deionized water, preferably deionized water.

[0037] In at least one specific embodiment, in step (4), the mass ratio of amorphous silica-alumina to urea is 0.45-0.55, preferably 0.5.

[0038] As another aspect of the present invention, it relates to food-grade white oil prepared by the above method.

[0039] In the present invention, urea and amorphous aluminosilicate are fully ground and decomposed into isocyanic acid and ammonia at 300°C. Isocyanic acid reacts with silanol groups, and the surface Si-OH becomes Si-NH2, and carbon dioxide is generated. The empty d orbital of the metal Pt atom and the lone pair of electrons of the amino nitrogen produce a chelating effect, and the Pt is anchored on the surface of the amorphous silica-alumina carrier. The interaction between the metal and the amino-modified amorphous silica-alumina carrier material is enhanced. During the calcination process, only short-range Pt atoms with close distances will gather into clusters, while long-range Pt atoms that are far away are not easy to gather due to the strong interaction force with the carrier surface. Urea modification increases the dispersion of active metals and hinders the growth of metal oxide particles. In addition, after the catalyst is reduced, the electron-donating amino group can stabilize the Pt 0 , enhancing its antioxidant properties and nano-metal cluster stability.

[0040] The food-grade white oil prepared by the invention has a water-white appearance, excellent oxidation stability and light and heat stability, a polycyclic aromatic hydrocarbon ultraviolet absorbance of ≯0.1cm, a color of +30, and a carbonized product passes, and other indicators meet the national standard GB / 1886.215-2016 for food-grade white oil No. 1-4. BRIEF DESCRIPTION OF THE DRAWINGS

[0041] Figure 1 : The process flow chart of producing food grade white oil according to the prior art. DETAILED DESCRIPTION

[0042] In order to have a clearer understanding of the technical features, purposes and beneficial effects of the present invention, the technical solution of the present invention is now described in detail below, which is not intended to limit the present invention.

[0043] In the prior art, the production process of food-grade white oil can refer to Figure 1 , mainly includes the following three sections:

[0044] Hydrogenation pre-refining: reaction pressure 10-15MPa, reaction temperature 350-390℃, volume space velocity 0.6-1.5 h -1 , hydrogen-oil ratio 300-800:1;

[0045] Hydroisomerization: reaction pressure 8-16MPa, reaction temperature 320-390℃, volume space velocity 0.6-1.5 h -1 , hydrogen-oil ratio 300-800:1;

[0046] White oil hydrogenation: reaction pressure 12-16MPa, reaction temperature 210-240℃, volume space velocity 0.5-1.0 h -1, hydrogen-to-oil ratio is 300-600:1. The specific process conditions can be adjusted according to the quality requirements of white oil products.

[0047] White oil hydrogenation catalyst needs to be reduced before playing a catalytic role. The reduction conditions are generally: hydrogen pressure 1.0-2.0MPa, reduction temperature 200-400℃, and reduction time 16h. The feed oil of the fixed bed white oil hydrogenation reactor should generally meet the requirements of aromatics content not more than 6wt%, nitrogen content not more than 2μg / g, and sulfur content not more than 10μg / g.

[0048] Preparation of white oil hydrogenation catalyst of the present invention

[0049] Example 1

[0050] This embodiment provides an amorphous silica-alumina supported white oil hydrogenation catalyst, the preparation process of which includes the following steps:

[0051] Step 1: Prepare a buffer solution by mixing 120 g of triethanolamine with 1200 g of deionized water and adding 48 g of diammonium phosphate to prepare a buffer solution.

[0052] Step 2: Add 400g aluminum sulfate 18hydrate to 600mL water, heat to 65°C and stir until dissolved. Add 398mL water to 198g silica sol with a particle size of 10-15nm, pH 3-5, and a concentration of 30wt%, and stir until the liquid is uniform and stable.

[0053] Step 3: Add the aluminum sulfate solution prepared in step 2 dropwise into the buffer solution prepared in step 1, maintain the water bath temperature at 70°C, stir while dropping, and the mechanical stirring speed is 600r / min. Continue stirring for 20 minutes after the addition is completed, add the diluted silica sol prepared in step 2, stir while dropping, and maintain the mechanical stirring speed at 600r / min. Continue stirring for 30 minutes after the addition is completed, and put the resulting mixed solution into a crystallization kettle, crystallize at 140°C for 24 hours, filter, wash to pH 7, dry at 60°C for 48 hours, and calcine at 500°C for 3 hours to obtain an amorphous silica-alumina carrier.

[0054] Step 4: Take 25 g of the amorphous silica-alumina carrier obtained in step 3, mix it with 12.5 g of urea, grind it into 320 mesh, place it in a sealed crucible and roast it at 150°C for 2 h and 300°C for 2 h.

[0055] Step 5: Dissolve 0.214 g of chloroplatinic acid in 28.5 g of deionized water to prepare a solution, use an equal volume of the solution to impregnate the amorphous silica-alumina support (20 g) obtained in step 4, and disperse it ultrasonically for 15 minutes, dry it at 100° C. for 5 hours, calcine it at 350° C. for 6 hours, and cool it to room temperature to obtain an amorphous silica-alumina support loaded with Pt;

[0056] Step 6: Dissolve 0.086 g of palladium nitrate in 28.5 g of deionized water to prepare a solution, use the solution to impregnate the above-mentioned platinum amorphous silica-alumina carrier, and ultrasonically disperse it for 15 minutes. Dry at 100°C for 5 hours, calcine at 350°C for 6 hours, and cool to room temperature to obtain a white oil hydrogenation catalyst.

[0057] The weight percentage of each component in the catalyst is SiO2:Al2O3:Pt:Pd=39:60.4:0.4:0.2. It is denoted as Cat-1.

[0058] Example 2

[0059] This example provides an amorphous silica-alumina supported white oil hydrogenation catalyst, the preparation process of which is the same as that of Example 1, except that the active metal is only supported with platinum, with a content of 0.6 wt%, and is denoted as Cat-2.

[0060] Example 3

[0061] This embodiment provides an amorphous silica-alumina supported white oil hydrogenation catalyst, the preparation process of which is the same as that of Example 2, except that after step 3, an equal volume of 0.333 mol / L phosphoric acid solution is used for impregnation, dried at 60°C for 24 hours, calcined at 500°C for 3 hours, and then the remaining steps are performed. This is denoted as Cat-3.

[0062] Comparative Example 1

[0063] The hydrotreating catalyst was prepared according to the method of Example 1, except that the amorphous silicon-alumina carrier used in the comparative example was prepared by the method provided in CN201710102791.2, which was designated as Cat-4.

[0064] Comparative Example 2

[0065] A hydrotreating catalyst was prepared according to the method of Example 1, except that the catalyst of the comparative example was directly loaded with active metals without amino modification, and was designated as Cat-5.

[0066] Comparative Example 3

[0067] The carrier was prepared according to the method of Example 1, except that the comparative catalyst was prepared by the method of CN102794203A. The catalyst was designated as Cat-6.

[0068] The following operations are carried out in the white oil hydrogenation reactor:

[0069] (1) Catalyst loading: several Φ3mm porcelain balls + 30mL white oil hydrogenation catalyst + several Φ3mm porcelain balls

[0070] (2) Catalyst reduction conditions: reduction temperature 250-400°C, pressure 1.0-2.0 MPa, hydrogen flow rate 20 L / h, reduction time 16 h.

[0071] The loading and sulfiding of the hydrotreating pre-refining catalyst can be carried out according to conventional methods, and the loading and reduction of the hydroisomerization catalyst can be carried out according to conventional methods.

[0072] The specific properties of the feedstock oil used in the examples of the present invention are shown in Table 1.

[0073] Table 1. Main properties of crude oil

[0074]

[0075] The three-stage reaction process conditions of the present invention are shown in Table 2.

[0076] Table 2. Hydrogenation process conditions

[0077]

[0078] Some properties of the product after hydrogenation pre-refining of the distillate are shown in Table 3.

[0079] Table 3. Some properties of hydrogenated pre-refined oil

[0080]

[0081] Some properties of the products of the above-mentioned refined oil and hydrocracking tail oil after hydroisomerization are shown in Table 4.

[0082] Table 4. Some properties of hydroisomerization oil

[0083]

[0084] The white oil hydrogenation catalyst prepared by the present invention was used to carry out white oil hydrogenation reaction with 1# minus second-line isomerized oil as raw material. The test results of the main indicators of the product are shown in Table 5.

[0085] Table 5. Test results of main indicators of 1# oil white oil products

[0086]

[0087] It can be seen from Table 5 that the hydrogenation effects of Cat-1 to Cat-3 on white oil of reduced second-line isomerized oil are better than those of Comparative Examples 1, 2 and 3, and the ultraviolet absorbance meets the requirement of <0.1 cm.

[0088] The white oil hydrogenation catalyst prepared by the present invention was used to carry out white oil hydrogenation reaction with 3# minus four-line isomerized oil as raw material. The test results of the main indicators of the product are shown in Table 6.

[0089] Table 6. Test results of main indicators of 3# oil white oil products

[0090]

[0091] It can be seen from Table 6 that the hydrogenation effects of Cat-1 to Cat-3 on white oil of reduced four-line isomerized oil are higher than those of Comparative Example 1, Comparative Example 2 and Comparative Example 3, and the ultraviolet absorbance meets the requirement of <0.1cm.

[0092] The white oil hydrogenation catalyst prepared by the present invention was used to carry out white oil hydrogenation reaction with 4# cracking tail oil isomerized oil as raw material. The test results of the main indicators of the product are shown in Table 7.

[0093] Table 7. Test results of main indicators of 4# oil white oil products

[0094]

[0095] It can be seen from Table 7 that the hydrogenation effects of Cat-1 to Cat-3 on the cracked tail oil isomerized oil are all higher than those of Comparative Example 1, Comparative Example 2 and Comparative Example 3, and the ultraviolet absorbance meets the requirement of <0.1 cm.

[0096] The catalyst of the present invention was used as a white oil hydrogenation catalyst, and the oil produced by linear isomerization and the oil produced by cracking tail oil isomerization were used as feed oils. The process conditions of the white oil hydrogenation reaction were investigated, and the product liquid recovery, product distribution and yield were optimized. The data are shown in Table 8.

[0097] Using Example 1 as the white oil hydrogenation catalyst, and the isomerized oil of the distillate oil and the cracking tail oil as the raw materials, the yield and distribution of each stage after white oil hydrogenation and product fractionation are shown in Table 8.

[0098] Table 8. White oil product distribution and yield

[0099]

[0100] Note: Liquid yield of white oil fraction = (product amount / feed amount) × 100%, white oil fraction yield = liquid yield of white oil fraction × fraction yield after fractionation

[0101] It can be seen from Table 8 that, by using the catalyst prepared by the present invention, the hydrogenation isomerization-white oil hydrogenation process can be used to produce food grade white oil products No. 1-4, with a total white oil yield of 79-90%, and light fractions such as naphtha, kerosene and diesel are produced as by-products.

[0102] Using Comparative Example 1 as a white oil hydrogenation catalyst, using distillate oil and cracking tail oil as raw materials, the yield and distribution of each stage after white oil hydrogenation and product fractionation are shown in Table 9.

[0103] Table 9. White oil product distribution and yield

[0104]

[0105] It can be seen from Table 9 that when the catalyst of Comparative Example 1 is used, the total yield of No. 1-4 white oil produced is reduced, and the light fraction increases.

[0106] The above-described embodiments are only preferred embodiments for fully illustrating the present invention, and the protection scope of the present invention is not limited thereto. Equivalent substitutions or changes made by those skilled in the art based on the present invention are within the protection scope of the present invention. The protection scope of the present invention shall be subject to the claims.

Claims

1. A hydrogenation method for producing food-grade white oil, wherein the pre-refined vacuum distillate oil or hydrocracking tail oil is subjected to a hydrogenation isomerization reaction to obtain an isomerized product oil, and the isomerized product oil is introduced into a fixed-bed white oil hydrogenation reactor, and the isomerized product oil undergoes olefin saturation and aromatic saturation reactions, characterized in that: A white oil hydrogenation catalyst is added to the fixed-bed white oil hydrogenation reactor, and the catalyst is an amorphous silicon-aluminum-based highly dispersed platinum-palladium white oil hydrogenation catalyst; The amorphous silicon-aluminum-based highly dispersed platinum-palladium white oil hydrogenation catalyst is prepared by the following method: (1) preparing a composite buffer using triethanolamine, deionized water and ammonium dihydrogen phosphate; (2) adding a silicon source and an aluminum source dropwise into the buffer solution to maintain a stable pH for precipitation; (3) crystallizing, washing, drying and calcining the solution obtained in step (2) to obtain an amorphous silicon-alumina carrier; (4) Modifying the amorphous silica-alumina support with urea: mixing and grinding the amorphous silica-alumina support with urea, and calcining the mixture in a closed crucible; (5) Platinum-palladium active metals are loaded onto the previously prepared carrier by an equal volume impregnation method, and then dried and calcined to obtain a highly dispersed platinum-palladium white oil hydrogenation catalyst.

2. The method according to claim 1, characterized in that In the step (4), the mass ratio of amorphous silica-alumina to urea is 0.45-0.55, and the closed calcination in the crucible means first heating to 150°C at a rate of 1°C / min and calcining for 2h, and then heating to 300°C at a rate of 1°C / min and calcining for 2h.

3. The method according to claim 1, characterized in that In the step (5), platinum is added in the form of any one of tetraammineplatinum nitrate, platinum acetate, platinum nitrate and chloroplatinic acid, and palladium is added in the form of any one of tetraamminepalladium nitrate, palladium nitrate, chloropalladic acid, palladium chloride and diamminepalladium dichloride.

4. The method according to claim 1, characterized in that In step (5), the content of platinum and palladium is 0.4wt% of platinum and 0.2wt% of palladium.

5. The method according to claim 1, characterized in that In step (1), the pH of the buffer solution is 11-12.

6. The method of claim 1, characterized in that In step (2), the reaction conditions are a temperature of 70° C. and a stable pH of 11.3-11.

8.

7. The method of claim 1, characterized in that In step (3), the crystallization conditions include: temperature of 140° C. and time of 24 h.

8. The method of claim 1, characterized in that In step (2), the silicon source is an acidic silica sol with a particle size of 10 nm.

9. The method of claim 8, characterized in that In step (2), the aluminum source is aluminum sulfate.

10. The method of claim 1, characterized in that The buffer solution in step (1) is prepared by mixing triethanolamine, deionized water and ammonium dihydrogen phosphate in a mass ratio of 5:50:

2.

11. The method of claim 9, characterized in that In step (2), the amounts of the acidic silica sol and aluminum sulfate are calculated based on the mass fractions of SiO2 and Al2O3, with the mass fraction of SiO2 accounting for 50%.

12. The method of claim 1, wherein: In the step (4), the mass ratio of amorphous silica-alumina to urea is 0.45-0.

55.

13. The method of claim 1, characterized in that In the step (4), the mass ratio of amorphous silica-alumina to urea is 0.

5.

14. Food grade white oil prepared using the method according to any one of claims 1 to 13.