Preparation method and application of super hydrophobic phosphogypsum powder in solid phase environment

By grinding phosphogypsum with sodium silicate and stearic acid in a solid-phase environment, superhydrophobic phosphogypsum powder is prepared, which solves the problem of water absorption and moisture absorption of phosphogypsum building materials and achieves low-cost, pollution-free hydrophobic modification. Suitable for construction and building materials applications.

CN116425438BActive Publication Date: 2024-10-22TAISHAN UNIV
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202310441479.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-04-23
Publication Date
2024-10-22
Estimated Expiration
2043-04-23

AI Technical Summary

Technical Problem

When using phosphogypsum in the prior art, its hydrophilicity makes building materials susceptible to moisture and mildew, and the treatment method consumes energy or increases costs. Moreover, traditional hydrophobic modification methods have problems with environmental pollution, cumbersome processes, and high costs.

Method used

In a solid-phase environment, phosphogypsum is ground with sodium silicate and stearic acid as raw materials. Through the substitution of sodium silicate and the adhesion of stearic acid, superhydrophobic phosphogypsum powder is prepared to achieve the hydrophobicity of phosphogypsum. modified.

Benefits of technology

It realizes the low-cost, pollution-free and simple process preparation of phosphogypsum, significantly improves its hydrophobicity, solves the problem of water absorption, moisture and mold of phosphogypsum building materials, and is suitable for the application of building materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116425438B_ABST
    Figure CN116425438B_ABST
Patent Text Reader

Abstract

The present invention discloses a method for preparing super-hydrophobic phosphogypsum powder under a solid phase environment, comprising the following steps: (1) selecting phosphogypsum, stearic acid and sodium silicate as raw materials; (2) first mixing phosphogypsum and sodium silicate, grinding, making phosphogypsum and sodium silicate fully contact, and obtaining a premix; (3) adding stearic acid to the premix, and continuing to grind, so that stearic acid fully adheres to the surface of phosphogypsum, and obtaining super-hydrophobic phosphogypsum powder. The present invention modifies the original phosphogypsum to obtain super-hydrophobic phosphogypsum, which has the property of not being easily affected by moisture. The super-hydrophobic phosphogypsum is used in building materials to replace the untreated original phosphogypsum with high impurities, which can well solve the problem of phosphogypsum building materials absorbing moisture and becoming moldy.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of utilization of phosphogypsum waste, and in particular to a preparation method and application of super-hydrophobic phosphogypsum powder in a solid phase environment. Background Art

[0002] Phosphogypsum is a solid waste of calcium sulfate discharged during the wet process of producing phosphoric acid. Every ton of phosphoric acid produced produces about four to six tons of phosphogypsum waste. Phosphogypsum can be used in the construction field, but because phosphogypsum is hydrophilic, building materials mixed with raw phosphogypsum are easily affected by moisture and mold.

[0003] In order to solve the hydrophilicity problem of phosphogypsum, it is currently necessary to perform simple treatment on phosphogypsum when using it. For example, phosphogypsum is calcined at high temperature to decompose calcium sulfate dihydrate into calcium sulfate hemihydrate and have gelling activity, but this treatment method consumes a lot of energy. Another example is that when phosphogypsum is used as a raw material for cementitious materials, various cement clinkers are added at the same time, which also increases the cost of phosphogypsum cementitious materials and is not conducive to the large-scale utilization of phosphogypsum.

[0004] The Chinese invention patent with application publication number CN113527911A discloses a method for surface hydroxylation and hydrophobic modification of phosphogypsum and phosphogypsum. The method first grinds the phosphogypsum and sieves it to obtain ultrafine phosphogypsum; then the ultrafine phosphogypsum is calcined in a gradient furnace to obtain ultrafine anhydrous phosphogypsum; in an aqueous phase, the ultrafine anhydrous phosphogypsum is hydroxylated with sodium hydroxide and sodium sulfate to obtain hydroxylated phosphogypsum; then in an ethanol phase, the hydroxylated phosphogypsum is surface modified with a surface modifier to obtain phosphogypsum with a hydrophobic surface. Although this method can effectively hydrophobically modify phosphogypsum, it has the following disadvantages:

[0005] (1) It needs to be prepared under aqueous conditions, which will cause secondary pollution to the environment; (2) The grinding, screening, calcination, hydroxylation and surface modification processes of phosphogypsum are cumbersome; (3) It needs to be calcined in a gradient furnace to obtain ultrafine anhydrous phosphogypsum, which is costly and not economical and practical; (4) This method only obtains hydrophobic phosphogypsum, and its hydrophobicity needs to be further improved. Summary of the invention

[0006] Based on the above technical problems, the present invention proposes a method for preparing super-hydrophobic phosphogypsum powder in a solid phase environment, and specific applications of the super-hydrophobic phosphogypsum powder prepared by the method.

[0007] The technical solution adopted by the present invention is:

[0008] A method for preparing super-hydrophobic phosphogypsum powder in a solid phase environment comprises the following steps:

[0009] (1) Selecting phosphogypsum, stearic acid and sodium silicate as raw materials;

[0010] (2) firstly mixing phosphogypsum and sodium silicate, and grinding them so that the phosphogypsum and sodium silicate are fully in contact with each other to obtain a premix;

[0011] (3) Stearic acid is added to the premix and the grinding is continued so that the stearic acid fully adheres to the surface of the phosphogypsum to obtain super hydrophobic phosphogypsum powder.

[0012] Preferably, in step (1): the phosphogypsum is original phosphogypsum, and the particle size of the phosphogypsum is in the range of 5-50 μm.

[0013] Preferably, in step (1), the weight ratio of the phosphogypsum, stearic acid and sodium silicate is 80-100:10-15:5-7.

[0014] More preferably, the weight ratio of the phosphogypsum, stearic acid and sodium silicate is 100:12:6.

[0015] Preferably, in step (2), the grinding time is 10-15 min.

[0016] Preferably, in step (3): the grinding time is 10-15 min.

[0017] The super-hydrophobic phosphogypsum powder prepared by the above method can be used in the preparation of building materials.

[0018] The beneficial technical effects of the present invention are:

[0019] The present invention modifies the original phosphogypsum to obtain super-hydrophobic phosphogypsum, which has the property of not being easily affected by moisture. The super-hydrophobic phosphogypsum is used in building materials to replace the untreated original phosphogypsum with high impurities, which can well solve the problem of phosphogypsum building materials absorbing moisture and becoming moldy.

[0020] The present invention first adds sodium silicate in a specific dosage ratio to the original phosphogypsum, and the silicate ions in the sodium silicate can replace the sulfate ions on the surface of the phosphogypsum to generate a Ca-SiO3 structure, and then a certain amount of stearic acid is further added for grinding. Due to the addition of sodium silicate in the early stage, the carboxyl structure in the stearic acid is more easily combined with the phosphogypsum, and the phosphogypsum powder is better wrapped by the stearic acid, so that the modified phosphogypsum reaches a super-hydrophobic state.

[0021] The present invention uses sodium silicate as an inorganic modifier and stearic acid as an organic modifier, the two are modified together, and a grinding method is adopted to prepare super-hydrophobic phosphogypsum, the hydrophobic modification effect is good, and the selected modifier has the advantages of low cost, economical and practical, non-toxic and pollution-free, good stability and the like.

[0022] The present invention prepares super-hydrophobic phosphogypsum in a solid phase environment, does not require an external water source, and is pollution-free to the environment; the present invention also has a simple preparation process, can quickly and conveniently prepare super-hydrophobic phosphogypsum, and can be widely applied to phosphogypsum-based building materials, has a low preparation cost, and is convenient for market promotion; the present invention can promote the utilization of phosphogypsum. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 It is a process flow chart of preparing super-hydrophobic phosphogypsum powder in a solid phase environment of the present invention;

[0024] Figure 2 This is an optical photograph of the contact angle of the super-hydrophobic phosphogypsum powder prepared in Example 1 of the present invention;

[0025] Figure 3 This is an optical photograph of the contact angle of the super-hydrophobic phosphogypsum powder prepared in Example 2 of the present invention;

[0026] Figure 4 This is the test state diagram of water droplets on the super-hydrophobic phosphogypsum surface;

[0027] Figure 5 This is a diagram showing the hydrophobicity test status of concrete building materials containing super-hydrophobic phosphogypsum;

[0028] Figure 6 XRD patterns of phosphogypsum (PG) and superhydrophobic phosphogypsum (SPG) prepared in Example 1 of the present invention;

[0029] Figure 7 The Fourier transform infrared spectra of phosphogypsum (PG) and super-hydrophobic phosphogypsum (SPG) prepared in Example 1 of the present invention. DETAILED DESCRIPTION

[0030] Terminology explanation:

[0031] Phosphogypsum: Phosphogypsum (PG) is a by-product of the phosphate fertilizer industry. For every ton of phosphoric acid produced, about 4-6 tons of phosphogypsum are produced. Phosphogypsum is grayish white or grayish black in color. Its main component is CaSO4·2H2O. Due to its strong acidity (pH<3) and high moisture content, only 15% of phosphogypsum products in the world are recycled as building materials, agricultural fertilizers or soil stabilizers.

[0032] Superhydrophobic: Superhydrophobic is a new type of material that can clean itself. Superhydrophobic material can achieve the effect of anti-fouling and waterproofing. At the same time, superhydrophobicity also has good applications in material anti-corrosion.

[0033] Super hydrophobic surface: refers to the contact angle between the material surface and the water droplet is greater than 150° and the rolling angle is less than 10°. The preparation of super hydrophobic surface generally needs to meet two conditions. One is that the material surface has very low surface energy, and the other is to prepare a rough micro-nano structure on the material surface. Because the material surface has low surface energy and rough micro-nano structure, water droplets can form round water beads on the material.

[0034] The present invention will be further described below in conjunction with specific embodiments.

[0035] Example 1

[0036] like Figure 1 As shown, 100g of phosphogypsum, 12g of stearic acid and 6g of sodium silicate are weighed as raw materials. The phosphogypsum is original phosphogypsum, and the particle size of the phosphogypsum ranges from 5 to 50 μm. Sodium silicate contains nine crystal waters, Na2SiO3·9H2O.

[0037] First, phosphogypsum and sodium silicate are mixed and ground for 10 minutes to allow the phosphogypsum and sodium silicate to fully contact each other to obtain a premix. Stearic acid is then added to the premix and ground for another 10 minutes to allow the stearic acid to fully adhere to the surface of the phosphogypsum to obtain super-hydrophobic phosphogypsum powder.

[0038] The optical photograph of the contact angle of the super-hydrophobic phosphogypsum powder prepared in this embodiment is as follows: Figure 2 As shown, the tested contact angle is 154.3°.

[0039] Example 2

[0040] 100g of phosphogypsum, 10g of stearic acid and 6g of sodium silicate are weighed as raw materials. The phosphogypsum is original phosphogypsum, and the particle size of the phosphogypsum ranges from 5 to 50 μm. Sodium silicate contains nine crystal waters, Na2SiO3·9H2O.

[0041] First, phosphogypsum and sodium silicate are mixed and ground for 10 minutes to allow the phosphogypsum and sodium silicate to fully contact each other to obtain a premix. Stearic acid is then added to the premix and ground for another 10 minutes to allow the stearic acid to fully adhere to the surface of the phosphogypsum to obtain super-hydrophobic phosphogypsum powder.

[0042] The optical photograph of the contact angle of the super-hydrophobic phosphogypsum powder prepared in this embodiment is as follows: Figure 2 As shown, the tested contact angle is 153.6°.

[0043] Example 3

[0044] 100g of phosphogypsum, 15g of stearic acid and 5g of sodium silicate are weighed as raw materials. The phosphogypsum is original phosphogypsum, and the particle size of the phosphogypsum ranges from 5 to 50 μm. Sodium silicate contains nine crystal waters, Na2SiO3·9H2O.

[0045] First, phosphogypsum and sodium silicate were mixed and ground for 12 minutes to allow the phosphogypsum and sodium silicate to fully contact each other to obtain a premix. Stearic acid was then added to the premix and ground for another 15 minutes to allow the stearic acid to fully adhere to the surface of the phosphogypsum to obtain super-hydrophobic phosphogypsum powder.

[0046] Example 4

[0047] 100g of phosphogypsum, 10g of stearic acid and 7g of sodium silicate are weighed as raw materials. The phosphogypsum is original phosphogypsum, and the particle size of the phosphogypsum ranges from 5 to 50 μm. Sodium silicate contains nine crystal waters, Na2SiO3·9H2O.

[0048] First, phosphogypsum and sodium silicate were mixed and ground for 15 minutes to allow the phosphogypsum and sodium silicate to fully contact each other to obtain a premix. Stearic acid was then added to the premix and ground for another 10 minutes to allow the stearic acid to fully adhere to the surface of the phosphogypsum to obtain super-hydrophobic phosphogypsum powder.

[0049] Example 5

[0050] 100g of phosphogypsum, 11g of stearic acid and 6g of sodium silicate are weighed as raw materials. The phosphogypsum is original phosphogypsum, and the particle size of the phosphogypsum ranges from 5 to 50 μm. Sodium silicate contains nine crystal waters, Na2SiO3·9H2O.

[0051] First, phosphogypsum and sodium silicate were mixed and ground for 12 minutes to allow the phosphogypsum and sodium silicate to fully contact each other to obtain a premix, and then stearic acid was added to the premix and ground for another 12 minutes to allow the stearic acid to fully adhere to the surface of the phosphogypsum to obtain super-hydrophobic phosphogypsum powder.

[0052] Comparative Example 1

[0053] 100 g of phosphogypsum and 12 g of stearic acid were weighed as raw materials for preparation. The phosphogypsum was original phosphogypsum, and the particle size of the phosphogypsum was in the range of 5-50 μm.

[0054] The phosphogypsum and stearic acid were mixed and ground for 10 minutes to allow the phosphogypsum and stearic acid to fully contact each other to obtain modified phosphogypsum powder. According to the test, the contact angle between the phosphogypsum powder and the water droplet was 123°, which could not reach the super-hydrophobic state.

[0055] Figure 4The figure is a diagram of the actual test state of water droplets on the surface of the super-hydrophobic phosphogypsum powder prepared in Example 1 of the present invention. It can also be clearly seen from the figure that the super-hydrophobic phosphogypsum powder prepared in the present invention has excellent hydrophobicity.

[0056] The super-hydrophobic phosphogypsum powder obtained in the above examples 1-5 can be further used to prepare building materials. Figure 5 This is an actual state diagram of the hydrophobicity test of the concrete building material prepared by the super-hydrophobic phosphogypsum powder of the present invention. It can also be seen from the figure that the concrete building material prepared by the super-hydrophobic phosphogypsum powder of the present invention has excellent hydrophobicity.

[0057] In addition, the present invention also performs XRD and FT-IR spectrum analysis on phosphogypsum (PG) and super hydrophobic phosphogypsum (SPG) prepared in Example 1. Figure 6 As shown in the figure, the crystal structure of PG and SPG was analyzed by XRD to determine their crystal composition. It was found that the main components of natural phosphogypsum are CaSO4·2H2O and SiO2. Compared with natural phosphogypsum (PG), the XRD spectrum of superhydrophobic phosphogypsum (SPG) did not change significantly. In addition, no diffraction peaks related to stearic acid molecules and sodium silicate appeared in the superhydrophobic phosphogypsum powder. This shows that the crystal structure of superhydrophobic phosphogypsum powder did not change during the dual modification process of stearic acid and sodium silicate.

[0058] Figure 7 The Fourier infrared spectra of phosphogypsum and superhydrophobic phosphogypsum are shown, where 3346.39 cm -1 The peaks on the left and right are related to the stretching vibration of the OH bond, 1635.20 cm -1 The absorption peaks around are caused by the deformation and vibration of water molecules. As can be seen from the figure, compared with natural phosphogypsum, the super-hydrophobic phosphogypsum powder has a peak at 3346.39 cm -1 and 1635.20cm -1 The intensity of the absorption peak at is significantly weakened, indicating that after modification, the number of hydroxyl groups in the superhydrophobic phosphogypsum powder is reduced and the water absorption is significantly weakened. It also shows that this modification is not just a physical modification. Figure 7 It can be seen that the super-hydrophobic phosphogypsum powder is at 2918.86cm -1 and 2849.67cm -1 Two new absorption peaks appeared at , which were caused by the stretching vibration of -CH3 and -CH2, proving that stearic acid had been successfully grafted onto the surface of phosphogypsum.

[0059] The parts not mentioned in the above methods can be realized by adopting or drawing on existing technologies.

[0060] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. An application of super-hydrophobic phosphogypsum powder in a solid phase environment in the preparation of building materials, wherein the preparation method of the super-hydrophobic phosphogypsum powder in the solid phase environment comprises the following steps: (1) Selecting phosphogypsum, stearic acid and sodium silicate as raw materials; (2) firstly mixing phosphogypsum and sodium silicate and grinding them so that the phosphogypsum and sodium silicate are fully in contact with each other to obtain a premix; (3) adding stearic acid to the premix and continuing to grind until the stearic acid is fully adhered to the surface of the phosphogypsum to obtain a super-hydrophobic phosphogypsum powder; In step (1), the phosphogypsum is original phosphogypsum, and the particle size of the phosphogypsum is in the range of 5-50 μm; the weight ratio of the phosphogypsum, stearic acid and sodium silicate is 100:12:6; In step (2): the grinding time is 10-15 min; In step (3): the grinding time is 10-15 min.

Citation Information

Patent Citations

  • Phosphogypsum surface hydroxylation and hydrophobic modification method and phosphogypsum

    CN113527911A

  • Hydrophobic phosphogypsum, and preparation method and application thereof

    CN101844884A

  • High-strength self-waterproof phosphogypsum roadbed material and preparation method thereof

    CN111320446A

  • Core-shell structure lightweight aggregate prepared by cold bonding method and preparation method thereof

    CN112194400A

  • Preparation method of three-dimensional super-hydrophobic gypsum with ultrahigh water cement ratio

    CN113480283A