UV-VIS radiation curing security inks for producing dichroic security features

By using UV-Vis irradiated cationic or hybrid curable security inks to print dichroic security features on valuable documents, the problem of insufficient mechanical resistance in high-speed production is solved, achieving a color rendering effect of blue under transmitted light and metallic yellow under incident light, while reducing production costs.

CN116438265BActive Publication Date: 2024-10-15SICPA HOLDING SA
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202180075725.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2020-11-10
Filing Date
2021-11-09
Publication Date
2024-10-15
Estimated Expiration
2041-11-09

AI Technical Summary

Technical Problem

Existing technologies struggle to produce high-speed, dichroic safety features on valuable documents that improve mechanical resistance and exhibit blue under transmitted light and metallic yellow under incident light. Furthermore, traditional methods are costly and lack sufficient mechanical resistance.

Method used

Security features are formed on valuable documents using UV-Vis radiation cationic curable security ink or UV-Vis radiation hybrid curable security ink, which contains approximately 7.5 wt% to approximately 20 wt% silver nanosheets, 45 wt% to approximately 80 wt% alicyclic epoxides and cationic curable compounds, and are formed by methods such as screen printing.

Benefits of technology

It achieves the production of dichroic safety features with improved mechanical resistance under high-speed printing, with significant color development effect, reduced production cost, and meets the needs of industrial printing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116438265B_ABST
    Figure CN116438265B_ABST
Patent Text Reader

Abstract

The present invention provides a UV-Vis radiation curable security ink for producing a security feature for protecting a valuable document, wherein the security feature appears blue when viewed under transmitted light and metallic yellow when viewed under incident light. The UV-Vis radiation curable security ink comprises a cationic curable or hybrid curable ink vehicle, and a silver nanosheet with a surface stabilizer of the general formula (I), wherein the residue R A is a C2-C4 alkyl group substituted with a hydroxyl group; the residue R B is selected from C1-C4 alkyl, and C2-C4 alkyl substituted with hydroxyl; and is of the general formula + NH2R C R D The ammonium cation, where the residue R C is a C2-C4 alkyl group substituted with a hydroxyl group; and the residue R D Selected from C1-C4 alkyl, and C2-C4 alkyl substituted with hydroxyl, #imgabs0#
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of security inks for producing dichroic security features for protecting value documents, wherein the dichroic security feature exhibits a first color when viewed in transmitted light and a second color different from the first color when viewed in incident light. Background Art

[0002] With the continuous improvement in the quality of color photocopies and prints and the attempt to protect security documents such as banknotes, valuable documents or cards, transportation tickets or cards, tax banderols, product labels, etc. that have an unreplicable effect to prevent counterfeiting, tampering or illegal copying, the conventional practice is to introduce various security features into these documents.

[0003] Security features used for security documents, for example, can generally be categorized as "covert" security features and "overt" security features. The protection provided by covert security features relies on the notion that such features are difficult to detect, typically requiring specialized instrumentation and knowledge for detection, whereas "overt" security features rely on the notion that they are easily detectable by unaided human senses, e.g. such features may be visible and / or detectable by touch, but still difficult to produce and / or replicate. However, the effectiveness of overt security features relies heavily on their easy identification as security features, since most users, particularly those who are not aware of the security feature of the document or article secured by the security feature in advance, will in fact perform security checks based solely on the security feature if they have actual knowledge of its existence and nature.

[0004] Dichroic security features play a special role in protecting valuable documents by presenting a first color when viewed under transmitted light and a second color different from the first color when viewed under incident light. In order to provide an eye-catching effect and attract the attention of laymen, the first color and the second color must have an attractive visual appearance, such as blue, metallic yellow, magenta, and green, and a significant color contrast (for example: blue / metallic yellow, green / metallic yellow, purple / metallic yellow).

[0005] A dichroic security feature that appears blue when viewed in transmitted light and metallic yellow when viewed in incident light can be obtained from silver flakes containing ink.

[0006] International patent application publication number WO2011064162A2 describes a solvent-based ink and a UV free radical curable ink containing silver flakes for producing a dichroic encryption or decorative element showing a gold / copper color in reflection and a blue color in transmission. The ink contains a high concentration of silver flakes, characterized in that the weight ratio between the silver flakes and the binder is 3:1.1. The high concentration of silver flakes in the ink used to obtain the encryption or decorative element described in WO2011064162A2 is detrimental to the mechanical resistance of the encryption or decorative element produced, and in addition, makes the production process of the element expensive. Further, the mechanical resistance of the encryption or decorative element described in WO2011064162A2 is weakened by using UV free radical curable inks or solvent-based inks, which provide a cured coating with limited mechanical resistance, as is well known to those skilled in the art. Since mechanical resistance is an essential property of a security element and the manufacturing method described in WO2011064162A2 is lengthy and rather expensive, the ink and the manufacturing method described therein are not suitable for industrial production on value documents of dichroic security features with acceptable mechanical resistance.

[0007] International patent application publication number WO2013186167A2 describes the use of a UV curable ink comprising silver flakes, a free radical curable binder and a large amount of organic solvent for coating a surface of a holographic structure. The coated holographic structure shows a blue color with a strong chromaticity in transmission and a yellow color with a low chromaticity in reflection on the embossed surface. Although the UV curable ink described in WO2013186167A2 contains a lower concentration of silver flakes than the UV radiation free radical curable ink described in WO2011064162A2, the ink is still not suitable for the industrial production of dichroic features on valuable documents because, on the one hand, the increased amount of organic solvent is not environmentally friendly and an additional air drying step is required before the UV curing step, and on the other hand, the coating obtained with the ink has limited mechanical resistance, as well as low chromaticity in reflection.

[0008] Typically, industrial printing of valuable documents requires high printing speeds of about 8'000 sheets / hour, wherein a large number of valuable documents are produced from each sheet of paper. For illustrative purposes, in the field of banknote printing, up to 55 valuable documents can be produced from one sheet of paper, each valuable document containing one or more security features. In order to be suitable for implementation on a production line, the production process of each printable security feature present on the valuable document must meet the high speed requirements of industrial printing of valuable documents.

[0009] Therefore, there remains a need for stable security inks for producing dichroic security features on value documents at high speeds (ie industrial speeds) that have improved mechanical resistance and appear blue when viewed in transmitted light and metallic yellow when viewed in incident light. Summary of the invention

[0010] It is therefore an object of the present invention to provide UV-Vis radiation cationically curable security inks and UV-Vis radiation hybrid curable security inks for producing dichroic security features on value documents at high speeds (i.e. industrial speeds), said dichroic security features having improved mechanical resistance and appearing blue when viewed under transmitted light and metallic yellow when viewed under incident light. This is achieved by the UV-VIS radiation curable security ink claimed herein, wherein said ink comprises:

[0011] a) about 7.5 wt-% to about 20 wt-% of silver nanoflakes, the silver nanoflakes having an average diameter in the range of 50 to 150 nm with a standard deviation of less than 60%, an average thickness in the range of 5 to 30 nm with a standard deviation of less than 50%, and an average aspect ratio greater than 2.0, wherein the average diameter is determined by transmission electron microscopy, and the average thickness is determined by transmission electron microscopy, and wherein the silver nanoflakes have a surface stabilizer of formula (I)

[0012]

[0013] in

[0014] Residue R A is a C2-C4 alkyl group substituted with a hydroxyl group;

[0015] Residue R B is selected from C1-C4 alkyl, and C2-C4 alkyl substituted with hydroxyl; and

[0016] Cat + For the general formula + NH2R C R D The ammonium cation, where the residue R C is a C2-C4 alkyl group substituted with a hydroxyl group; and the residue R D is selected from C1-C4 alkyl, and C2-C4 alkyl substituted with hydroxyl;

[0017] b) about 45 wt-% to about 80 wt-% of a cycloaliphatic epoxide, or a mixture of a cycloaliphatic epoxide and one or more UV-Vis radiation curable compounds;

[0018] c) one or more cationic photoinitiators;

[0019] d) a perfluoropolyether surfactant functionalized with one or more functional groups selected from the group consisting of hydroxyl, acrylate, methacrylate, and trialkoxysilyl;

[0020] e) from about 3 wt-% to about 12 wt-% of a polyvinyl chloride copolymer, the polyvinyl chloride copolymer comprising at least 60 wt-% vinyl chloride; and optionally

[0021] f) up to about 25 wt-% of an organic solvent;

[0022] The weight percentages are based on the total weight of the UV-Vis radiation curable security ink.

[0023] According to another aspect of the invention, a method for producing a security feature for protecting a valuable document, wherein the security feature appears blue when viewed in transmitted light and metallic yellow when viewed in incident light, comprises the following steps:

[0024] A) printing a UV-Vis radiation curable security ink as claimed and described herein onto a transparent or partially transparent area of ​​a substrate of a value document to provide an ink layer, preferably by screen printing, rotogravure printing, or flexographic printing; and

[0025] B) UV-Vis curing of the ink layer obtained in step A) to form a security feature. DETAILED DESCRIPTION

[0026] definition

[0027] The following definitions are intended to clarify the meaning of the terms discussed in the specification and recited in the claims.

[0028] As used herein, the indefinite article "a" or "an" refers to one or more than one, and does not necessarily limit its designated noun to the singular.

[0029] As used herein, the term "about" means that the amount or value in question can be a specified certain value or some other value in the vicinity thereof. Typically, the term "about" representing a specific value is intended to represent a range within ±5% of the value. As an example, the phrase "about 100" represents a range of 100 ± 5, that is, a range from 95 to 105. Preferably, the range represented by the term "about" represents a range within ±3% of the value, more preferably ±1%. Typically, when the term "about" is used, it is expected that similar results or effects according to the present invention can be obtained within a range of ±5% of the specified value.

[0030] As used herein, the term "and / or" means that all or only one of the elements of the group may be present. For example, "A and / or B" means "only A, or only B, or both A and B". In the case of "only A", the term also covers the possibility that B does not exist, that is, "only A, but not B".

[0031] The term "comprising" as used herein is intended to be non-exclusive and open-ended. Thus, for example, a solution comprising compound A may include other compounds in addition to A. However, as a specific embodiment thereof, the term "comprising" also encompasses the more restrictive meanings of "consisting essentially of" and "consisting of", so that, for example, "a solution comprising A, B and optionally C" may also consist (essentially) of A and B or (essentially) of A, B and C.

[0032] Insofar as the present description refers to “preferred” embodiments / features, combinations of these “preferred” embodiments / features shall also be deemed disclosed, insofar as the specific combination of “preferred” embodiments / features makes technical sense.

[0033] As used herein, the term "one or more" means one, two, three, four, etc.

[0034] The terms "UV-Vis curable" and "UV-Vis curing" refer to radiation curing by means of photopolymerization under the influence of radiation having a wavelength component in the UV or in the UV and visible part of the electromagnetic spectrum (typically, 100 nm to 800 nm, preferably between 150 and 600 nm, and more preferably between 200 and 400 nm).

[0035] Surprisingly, a UV-Vis radiation curable security ink has been found comprising:

[0036] a) about 7.5 wt-% to about 20 wt-% of silver nanoflakes, the silver nanoflakes having an average diameter in the range of 50 to 150 nm with a standard deviation of less than 60%, an average thickness in the range of 5 to 30 nm with a standard deviation of less than 50%, and an average aspect ratio greater than 2.0, wherein the average diameter is determined by transmission electron microscopy, and the average thickness is determined by transmission electron microscopy, and wherein the silver nanoflakes have a surface stabilizer of formula (I)

[0037]

[0038] in

[0039] Residue R A is a C2-C4 alkyl group substituted with a hydroxyl group;

[0040] Residue R B is selected from C1-C4 alkyl, and C2-C4 alkyl substituted with hydroxyl; and

[0041] Cat + For the general formula + NH2R C RD The ammonium cation,

[0042] The residue R C is a C2-C4 alkyl group substituted with a hydroxy group; and

[0043] Residue R D is selected from C1-C4 alkyl, and C2-C4 alkyl substituted with hydroxyl;

[0044] b) about 45 wt-% to about 80 wt-% of a cycloaliphatic epoxide, or a mixture of a cycloaliphatic epoxide and one or more UV-Vis radiation curable compounds;

[0045] c) one or more cationic photoinitiators;

[0046] d) a perfluoropolyether surfactant functionalized with one or more functional groups selected from the group consisting of hydroxyl, acrylate, methacrylate, and trialkoxysilyl;

[0047] e) from about 3 wt-% to about 12 wt-% of a polyvinyl chloride copolymer, the polyvinyl chloride copolymer comprising at least 60 wt-% vinyl chloride; and optionally

[0048] f) up to about 25 wt-% of an organic solvent; the weight percentages are based on the total weight of the UV-Vis radiation curable security ink, enabling convenient and cost-effective production of security features with improved mechanical resistance and showing a blue color in transmitted light and a metallic yellow color in incident light. The combination of specific silver nanoflakes with a surface stabilizer of the general formula (I) described herein and a specific ink vehicle described herein allows the silver nanoflakes contained in the ink layer obtained by printing the security ink according to the invention to conveniently migrate from the mass of the ink layer to the interface between the ink layer and the air and to the interface between the ink layer and the substrate and to align at said interfaces to form a thin reflective layer, thereby producing a metallic yellow color in reflection and a blue color in transmission, regardless of the thickness of the printed ink layer. The advantageous color development of a metallic yellow color in reflection and a blue color in transmission cannot be achieved with the inks described in the prior art. The cationic curable binder or hybrid curable binder contained by the UV-Vis radiation curable security ink claimed herein provides a dichroic security feature with high mechanical resistance obtained by said ink. The attractive visual appearance and the contrast between the blue color presented in transmitted light and the metallic yellow color presented in incident light make the security feature produced with the ink according to the invention obvious, thereby drawing the attention of the layman to the security feature and facilitating the discovery and recognition of the security feature on a valuable document and facilitating the identification of a valuable document comprising the security feature. The UV-Vis radiation curable ink according to the invention has an outstanding storage stability. Therefore, the UV-Vis radiation curable security ink according to the invention is stable, meets the high speed requirements of industrial printing of valuable documents, and provides a dichroic security feature with an attractive visual appearance, high value recognition and good mechanical resistance.

[0049] The security feature made with the UV-Vis radiation curable security ink claimed herein appears blue in transmitted light, i.e. when viewed in transmission. For the purposes of the present invention, viewing in transmitted light means illuminating the security feature from one side, for example by holding the security feature against daylight or in front of a light source, and viewing from the opposite side. Independently of the side on which the security feature is viewed in transmitted light, a blue color is observed. For the purposes of the present invention, a security feature that appears blue is one that appears blue characterized by a chromaticity value C* (corresponding to a measure of color intensity or color saturation) above 20. An intense to very intense blue color is characterized by a chromaticity value C* above 30. The chromaticity value C* is calculated from the a* and b* values ​​according to the CIELAB (1976) color space, where

[0050]

[0051] The a* and b* values ​​were measured in transmitted light using a Datacolor 650 spectrophotometer (parameters: integrating sphere, diffuse illumination (pulsed xenon D65) and 8° observation, analyzer SP2000 with dual 256 diode array for 360-700 nm wavelength range, transmission sampling aperture size 22 mm).

[0052] The security feature made with the UV-Vis radiation curable security ink claimed herein appears metallic yellow or gold when viewed in incident light, i.e. in reflection. In the present patent application, the terms "metallic yellow" and "gold" may be used interchangeably. For the purposes of the present invention, "viewed in incident light" means that the security feature is illuminated from the side printed with the security ink claimed herein, and is viewed from the same side. For the purposes of the present invention, a security feature that appears metallic yellow or gold means a security feature that appears yellow characterized by a chromaticity value C* (corresponding to a measure of color intensity or color saturation) calculated from the a* and b* values ​​according to the CIELAB (1976) color space, higher than 20, wherein

[0053]

[0054] And wherein the a* and b* values ​​of the security feature are measured using a goniometer (Goniospektrometer Codec WI-105&5 from Phyma GmbH Austria) at an illumination angle of 22.5° from 0° to normal.

[0055] The UV-Vis radiation curable security ink claimed and described herein is preferably selected from screen printing security inks, rotogravure printing security inks, and flexographic printing security inks. Preferably, the UV-Vis radiation curable security ink claimed herein is characterized by a viscosity at 25°C between about 50 mPas and about 2000 mPas, measured at 100 rpm using a Brookfield viscometer (model "DV-I Prime) equipped with a spindle S27, or the viscometer is equipped with a spindle S21 at 50 rpm to measure a viscosity between 500 and 2000 mPas, and the viscometer is equipped with a spindle S21 at 100 rpm to measure a viscosity equal to or lower than 500 mPas. The UV-Vis radiation curable security ink claimed herein is characterized by a viscosity at 25°C between about 50 mPas and about 1000 mPas, preferably a viscosity at 25°C between about 100 mPas and about 1000 mPas.

[0056] As known to those skilled in the art, the term rotogravure refers to a printing method described, for example, in Handbook of Print Media, Helmut Kipphan, Springer Edition, page 48. Rotogravure is a printing method in which image elements are engraved into the surface of a cylinder. The non-image area is at a constant original level. Before printing, the entire printing plate (non-printing and printing elements) is inked and filled with ink. Before printing, the ink is removed from the non-image by a wiper or a blade so that the ink remains only in the cells. The image is transferred from the cells to the substrate by a pressure generally in the range of 2 to 4 bars and by the adhesion between the substrate and the ink. The term rotogravure does not include intaglio printing methods (also referred to in the art as engraved steel molds or copperplate printing methods) that rely, for example, on different types of inks.

[0057] The flexography printing method preferably uses a unit with a chambered doctor blade, an anilox roller and a plate cylinder. The anilox roller advantageously has small cells, whose volume and / or density determine the speed of ink or varnish application. The chambered doctor blade is pressed against the anilox roller, filling the cells and scraping off excess ink or varnish at the same time. The anilox roller transfers the ink to the plate cylinder, which ultimately transfers the ink to the substrate. The plate cylinder can be made of a polymer material or an elastomeric material. Polymers are mainly used as photopolymers in the plate and sometimes as seamless coatings on sleeves. Photopolymer plates are made of photosensitive polymers that are hardened by ultraviolet (UV) light. The photopolymer plate is cut into the required size and placed in a UV light exposure unit. One side of the plate is completely exposed to UV light to harden or cure the substrate of the plate. The plate is then turned over, the negative of the job is mounted on the uncured side, and the plate is then further exposed to UV light. This hardens the plate in the image area. The plate is then processed to remove the unhardened photopolymer from the non-image areas, which reduces the plate surface in these non-image areas. After processing, the plate is dried and given a post-exposure dose of UV light to cure the entire plate. The preparation of flexographic plate cylinders is described in Printing Technology, JM Adams and PADolin, Delmar Thomson Learning, 5th edition, pages 359-360.

[0058] As known to those skilled in the art, screen printing (also known in the art as silkscreen printing) is a printing technique that typically uses a screen made of a woven mesh to support an ink-blocking stencil. The attached stencil forms open areas of a grid that transfer ink to a substrate as a sharp-edged image. A squeegee moves across the screen with the ink-blocking stencil, forcing the ink to pass through the wires of the woven mesh in the open areas. A notable feature of screen printing is that a greater thickness of ink can be applied to a substrate than with other printing techniques. Therefore, when an ink deposit having a thickness of about 10 to 50 μm or more is required, which cannot be (easily) achieved by other printing techniques, screen printing is also preferred. Typically, a screen is made of a porous piece of finely woven fabric called a mesh stretched on a frame such as aluminum or wood. Most current meshes are made of artificial materials such as synthetic wire or steel wire. The preferred synthetic material is nylon or polyester wire.

[0059] In addition to wire meshes made of woven meshes based on synthetic or metallic wires, wire meshes are also made of solid metal sheets having a grid of holes. Such wire meshes are prepared by a method comprising electrolytically forming a metal wire mesh by forming a wire mesh skeleton on a substrate provided with a separating agent in a first electrolytic bath, extracting the formed wire mesh skeleton from the substrate, and subjecting the wire mesh skeleton to electrolysis in a second electrolytic bath to deposit a metal on the skeleton.

[0060] There are three types of screen printers, flatbed, drum and rotary screen printers. Flatbed and drum screen printers are similar in that they both use a flatbed screen and a three-step reciprocating process to perform the printing operation. The screen is first moved into position above the substrate, then a squeegee is pressed against the mesh and pulled over the image area, and the screen is then lifted from the substrate to complete the process. With a flatbed printer, the substrate to be printed is typically placed on a horizontal print bed parallel to the screen. With a drum printer, the substrate is mounted on a drum. Flatbed and drum screen printing processes are discontinuous processes, so speeds are limited, typically a maximum of 45m / minute in a web, or 3'000 sheets / hour in a sheet-fed process.

[0061] In contrast, rotary screen printers are designed for continuous, high-speed printing. The screen used on a rotary screen printer is a thin metal cylinder, such as is usually obtained using the electroforming method described above or made from braided steel wire. The open cylinder is capped at both ends and mounted into a block on the side of the press. During printing, ink is pumped into one end of the cylinder so that a fresh supply is constantly maintained. A doctor blade is fixed inside the rotary screen and the doctor blade pressure is maintained and adjusted to allow a good and constant print quality. The advantage of a rotary screen printer is that speeds can easily reach 150 m / min in a web-fed or 10'000 sheets / hour in a sheet-fed method.

[0062] Screen printing is further described in, for example, The Printing Ink Manual, RH Leach and RH Pierce, Springer Edition, 5th edition, pages 58-62, in Printing Technology, JA Adams and PA Dolin, Delmar Thomson Learning, 5th edition, pages 293-328 and in Handbook of Print Media, H. Kipphan, Springer, pages 409-422 and 498-499.

[0063] More preferably, the UV-Vis radiation curable security ink claimed and described herein is a screen printing security ink. Such UV-Vis radiation curable screen printing security ink is particularly useful for the industrial production of dichroic security features on value documents, as it enables the printing of dichroic security features with a large thickness of at least about 4 μm at very high speeds.

[0064] The UV-VIS radiation curable ink claimed and described herein comprises a) about 7.5 wt-% to about 20 wt-%, preferably about 7.5 wt-% to about 15 wt-%, more preferably about 10 wt-% to about 13 wt-% of silver nanoflakes, said silver nanoflakes having an average diameter in the range of 50 to 150 nm with a standard deviation of less than 60%, an average thickness in the range of 5 to 30 nm with a standard deviation of less than 50%, and an average aspect ratio above 2.0, wherein the average diameter is determined by transmission electron microscopy, and the average thickness is determined by transmission electron microscopy, and wherein the silver nanoflakes carry a surface stabilizer of the general formula (I)

[0065]

[0066] in

[0067] Residue R A is a C2-C4 alkyl group substituted with a hydroxyl group;

[0068] Residue R B is selected from C1-C4 alkyl, and C2-C4 alkyl substituted with hydroxyl; and

[0069] Cat + For the general formula + NH2R C R D The ammonium cation,

[0070] The residue R C is a C2-C4 alkyl group substituted with a hydroxy group; and

[0071] Residue R D Selected from C1-C4 alkyl, and C2-C4 alkyl substituted with hydroxyl.

[0072] The silver nanoflakes with the surface stabilizer of the general formula (I) described herein can be easily dispersed in the binder of the UV-Vis radiation curable security ink claimed herein. During printing, the silver nanoflakes described herein migrate from the bulk of the ink layer obtained with the UV-Vis radiation curable security ink claimed herein to the interface between the ink layer and the air and the interface between the ink layer and the substrate and arrange themselves at said interfaces to form a thin layer of silver nanoflakes, resulting in an advantageous color development of a metallic yellow color observed under incident light. This property of the UV-Vis radiation curable security ink claimed herein is particularly advantageous because, on the one hand, the time required for the color development of the metallic yellow color is compatible with the high-speed requirements of industrial printing of valuable documents and, on the other hand, it enables the production of dichroic security features with inks containing silver nanoflakes in an amount as low as 7.5 wt-%, which greatly reduces the production costs, especially for dichroic security features with a large thickness of at least about 4 μm. Depending on the thickness of the dichroic security feature to be produced and the composition of the ink vehicle, the amount of silver nanoflakes in the UV-Vis radiation curable security ink can be adjusted to allow rapid development of a metallic yellow color under reflected light without affecting the hue and chroma of the blue color under transmitted light.

[0073] The silver nanosheets included in the UV-Vis can be in the form of disks, regular hexagons, triangles (especially equilateral triangles) and truncated triangles (especially truncated equilateral triangles), or mixtures thereof. They are preferably in the form of disks, truncated triangles, hexagons, or mixtures thereof.

[0074] The average diameter of the silver nanosheets is in the range of 50 to 150 nm, preferably 60 to 140 nm, more preferably 70 to 120 nm, with a standard deviation of less than 60%, preferably less than 50%. The diameter of the silver nanosheets is the longest dimension of the silver nanosheets and corresponds to the maximum dimension of the silver nanosheets when oriented parallel to the plane of the transmission electron microscope (TEM) image. As used herein, the term "average diameter of silver nanosheets" refers to the average diameter determined by transmission electron microscopy (TEM) using Fiji image analysis software based on the measurement of at least 300 randomly selected silver nanosheets oriented parallel to the plane of the transmission electron microscope (TEM) image, wherein the diameter of the silver nanosheets is the maximum dimension of the silver nanosheets oriented parallel to the plane of the transmission electron microscope image (TEM). TEM analysis was performed in bright field mode using an EM 910 instrument from ZEISS at an electron beam acceleration voltage of 100 kV. TEM analysis was performed using a dispersion of silver nanosheets at a suitable concentration, preferably less than 24.1 wt-%, in isopropanol.

[0075] The average thickness of the silver nanosheets is in the range of 5 to 30 nm, preferably 7 to 25 nm, more preferably 8 to 25 nm, with a standard deviation of less than 50%, preferably less than 30%. The thickness of the silver nanosheets is the shortest dimension of the nanosheets and corresponds to the maximum thickness of the silver nanosheets. As used herein, the term "average thickness of the silver nanosheets" refers to the average thickness determined by transmission electron microscopy (TEM) based on manual measurements of at least 50 randomly selected silver nanosheets oriented perpendicular to the plane of the TEM image, wherein the thickness of the silver nanosheets is the maximum thickness of the silver nanosheets. TEM analysis was performed in bright field mode using an EM 910 instrument from ZEISS at an electron beam acceleration voltage of 100 kV. TEM analysis was performed using a dispersion of silver nanosheets at a suitable concentration, preferably less than 24.1 wt-%, in isopropanol.

[0076] The average aspect ratio of the silver nanoplatelets (defined as the ratio between the average diameter and the average thickness) is greater than 2.0, preferably greater than 2.2, and more preferably greater than 2.5.

[0077] Preferably, the average diameter of the silver nanosheets is in the range of 70 to 120 nm with a standard deviation of less than 50%, the average thickness of the silver nanosheets is in the range of 8 to 25 nm with a standard deviation of less than 30%, and the average aspect ratio of the silver nanosheets is higher than 2.5.

[0078] The silver nanoplatelets used in the UV-Vis radiation curable ink described herein are characterized by having a maximum wavelength absorption maximum between 560 and 800 nm, preferably between 580 and 800 nm, and most preferably between 600 and 800 nm. The Varian Cary 50 UV-Vis spectrophotometer was used to measure the silver concentration at about 5*10 -5 The maximum absorption maximum at the highest wavelength is measured in water with a concentration of 1.5 M (mol / l). The full width at half maximum (FWHM) value of the absorption maximum is in the range of 50 to 500 nm, preferably 70 to 450 nm, and more preferably 80 to 450 nm. The molar extinction coefficient of the silver nanosheets measured at the maximum absorption maximum at the highest wavelength is higher than 4000 L / (cm*mol Ag ), especially higher than 5000L / (cm*mol Ag ), very particularly above 6000 L / (cm*mol Ag ).

[0079] The UV-VIS radiation curable ink claimed herein comprises silver nanosheets having a surface stabilizer of the general formula (I)

[0080]

[0081] The residue R A is a C2-C4 alkyl group substituted with a hydroxyl group; the residue R B is selected from C1-C4 alkyl, and C2-C4 alkyl substituted with hydroxyl; and Cat + For the general formula + NH2R C R D The ammonium cation, where the residue R C is a C2-C4 alkyl group substituted with a hydroxyl group; and the residue R D The surface stabilizer of formula (I) is selected from C1-C4 alkyl, and C2-C4 alkyl substituted with hydroxyl. Without being bound by this theory, it is believed that the surface stabilizer of formula (I) helps to promote the migration of silver nanosheets from the bulk of the ink layer obtained with the safety ink claimed herein at the interface between the ink layer and the air and at the interface between the ink layer and the substrate, in addition to preventing the agglomeration and sedimentation of the silver nanosheets in the safety ink claimed herein.

[0082] The surface stabilizer of formula (I) may be present in an amount of about 0.5% to about 5%, preferably about 0.5% to about 4%, and more preferably about 3%, based on the percentage (wt-%) of the silver nanoplatelets.

[0083] As used herein, the term "C1-C4 alkyl" refers to a saturated straight or branched monovalent hydrocarbon group of 1 to 4 carbon atoms (C1-C4). Examples of C1-C4 alkyl groups include methyl (Me, -CH3), ethyl (Et, -CH2CH3), 1-propyl (n-Pr, n-propyl, -CH2CH2CH3), 2-propyl (i-Pr, isopropyl, -CH(CH3)2), 1-butyl (n-Bu, n-butyl, -CH2CH2CH2CH3), 2-methyl-1-propyl (i-Bu, isobutyl, -CH2CH(CH3)2), 2-butyl (s-Bu, sec-butyl, -CH(CH3)CH2CH3) and 2-methyl-2-propyl (t-Bu, tert-butyl, -C(CH3)3).

[0084] The term "C2-C4 alkyl group substituted with a hydroxyl group" refers to a straight or branched alkyl group having 2 to 4 carbon atoms, which is substituted with a hydroxyl group (-OH). The C2-C4 alkyl group may be substituted with one or two hydroxyl groups.

[0085] In the general formula (I), the residue R A may be a C2-C4 alkyl group substituted with two hydroxy groups, and the residue R B It may be a C1-C4 alkyl group.

[0086] In a preferred embodiment according to the present invention, the residue R A and R B are independently C2-C4-alkyl substituted with hydroxyl groups, preferably with one hydroxyl group. A and R B The residue R is independently selected from the group consisting of: –CH2CH2OH, –CH2CH(OH)CH3, –CH2CH2CH2OH, –CH(CH3)(CH2OH), –CH2CH(OH)CH2CH3, –CH2CH2CH(OH)CH3, –CH2CH2CH2OH, –CH(CH3)CH(OH)CH3, –CH(CH2OH)CH2CH3, –CH(CH3)CH2CH2OH, –CH2CH(CH2OH)CH3, –CH2C(CH3)(OH)CH3, –CH2CH(CH3)CH2(OH), –CH2C(OH)(CH3)2, –CH2C(CH3)(CH2OH, more preferably selected from the group consisting of: –CH2CH2OH, –CH2CH(OH)CH3, and –CH2CH2CH2OH. A and R B It can be the same, or it can be different.

[0087] In the general formula (I), the residue RC may be a C2-C4 alkyl group substituted with two hydroxy groups, and the residue R D It may be a C1-C4 alkyl group.

[0088] In a preferred embodiment according to the present invention, the residue R C and R D are independently C2-C4-alkyl substituted with hydroxyl groups, preferably with one hydroxyl group. C and R D The residue R is independently selected from the group consisting of: –CH2CH2OH, –CH2CH(OH)CH3, –CH2CH2CH2OH, –CH(CH3)(CH2OH), –CH2CH(OH)CH2CH3, –CH2CH2CH(OH)CH3, –CH2CH2CH2OH, –CH(CH3)CH(OH)CH3, –CH(CH2OH)CH2CH3, –CH(CH3)CH2CH2OH, –CH2CH(CH2OH)CH3, –CH2C(CH3)(OH)CH3, –CH2CH(CH3)CH2(OH), –CH2C(OH)(CH3)2, –CH2C(CH3)(CH2OH, more preferably selected from the group consisting of: –CH2CH2OH, –CH2CH(OH)CH3, and –CH2CH2CH2OH. C and R D It can be the same, or it can be different.

[0089] Preferably, in the general formula (I), the residue R A , R B , R C and R D are independently C2-C4 alkyl substituted with one hydroxyl group. More preferably, in the general formula (I), the residue R A , R B , R C and R D are independently selected from the group consisting of: -CH2CH2OH, -CH2CH(OH)CH3, and -CH2CH2CH2OH. Even more preferably, in general formula (I), the residue R A , R B , R C and R D It stands for –CH2CH2OH.

[0090] In order to prevent the silver nanosheets from agglomerating and settling during storage, the silver nanosheets may be provided with a further surface stabilizer on their surface.

[0091] In a preferred embodiment, the silver nanosheets carry on their surface a further surface stabilizer of the general formula (II)

[0092]

[0093] in

[0094] R 1 H, C1-C 18 Alkyl, phenyl, C1-C8 alkylphenyl, or CH2COOH;

[0095] R 2 , R 3 , R 4 , R 5 , R 6 and R 7 are independently H, C1-C8 alkyl, or phenyl;

[0096] Y is O or NR 8 ;

[0097] R 8 is H, or C1-C8 alkyl;

[0098] k1 is an integer in the range of 1 to 500;

[0099] k2 and k3 are independently 0 or an integer in the range of 1 to 250;

[0100] k4 is 0 or 1; and

[0101] k5 is an integer in the range of 1 to 5. Preferably, in the general formula (II), Y represents O. Also preferably, in the general formula (II), k4 is 0.

[0102] The average molecular weight (Mn) of the surface stabilizer of the general formula (II) is preferably 1000 to 20000 [g / mol], and more preferably 1000 to 10000 [g / mol], and most preferably 1000 to 6000 [g / mol].

[0103] If the surface stabilizer of the formula (I) comprises, for example, ethylene oxide units (EO) and propylene oxide units (PO), the sequence of (EO) and (PO) can be fixed (block copolymers) or not (random copolymers).

[0104] Preferably, in the general formula (II), R 1 H, or C1-C 18 Alkyl, R 2 , R 3 , R 4 , R 5 , R 6 and R7 are independently H, CH3, or C2H5, k1 is an integer in the range of 22 to 450, k2 and k3 are independently 0, or an integer in the range of 1 to 250, k4 is 0, or 1, and k5 is an integer in the range of 1 to 5. More preferably, in the general formula (II), R 1 is H, or C1-C4 alkyl, R 2 , R 3 , R 4 , R 5 , R 6 and R 7 They are independently H or CH3, k1 is an integer in the range of 22-450, k2 and k3 are independently 0 or an integer in the range of 1-100, k4 is 0, and k5 is an integer in the range of 1-4.

[0105] The most preferred surface stabilizer of formula (II) has the formula (II-a)

[0106]

[0107] in

[0108] R 1 is H, or C1-C8 alkyl, especially H, or CH3, and

[0109] k1 is an integer in the range of 22-450, especially 22-150.

[0110] Preferred surface stabilizers of formula (II) are derived from the average molecular weight (M n ) is 2000 to 6000 MPEG thiols (poly (ethylene glycol) methyl ether thiols), for example, MPEG 2000 thiol, MPEG 3000 thiol, MPEG 4000 thiol, MPEG 5000 thiol, MPEG 6000 thiol, with an average M n PEG thiols (O-(2-mercaptoethyl)-poly(ethylene glycol)) of 2000 to 6000, for example, PEG 2000 thiol, PEG 3000 thiol, PEG 4000 thiol, PEG 5000 thiol, PEG 6000 thiol.

[0111] The silver nanosheets contained in the security ink may further carry a surface stabilizer, and the surface stabilizer is a polymer or copolymer described in WO200674969A1, which can be obtained by a method comprising the following steps:

[0112] i-1) In a first step, one or more ethylenically unsaturated monomers are polymerized in the presence of at least one nitroxyl ether having the following structural units:

[0113]

[0114] wherein X represents a group having at least one carbon atom and such that a free radical X· originating from X is capable of initiating polymerization; or

[0115] i-2) In the first step, at least one stable nitroxyl radical and a free radical initiator, polymerizing one or more ethylenically unsaturated monomers;

[0116] wherein at least one monomer used in step i-1) or i-2) is a C1-C6 alkyl or hydroxy C1-C6 alkyl ester of acrylic acid or methacrylic acid; and optionally

[0117] ii) A second step comprising modifying the polymer or copolymer prepared in i-1) or i-2) by transesterification, amidation, hydrolysis or anhydride modification or a combination thereof.

[0118] The monomer in step i-1) or i-2) is preferably selected from 4-vinyl-pyridine or pyridinium ion, 2-vinyl-pyridine or pyridinium ion, 1-vinyl-imidazole or imidazolinium ion, or a monomer of the formula CH2=C(R a )-(C=Z)-R b of compounds, wherein

[0119] R a is hydrogen or methyl;

[0120] R b NH2, O - (Me + ), unsubstituted C1-C 18 Alkoxy, C2-C 100 Alkoxy or hydroxy substituted C1-C 18 Alkoxy, unsubstituted C1-C 18 Alkylamino, unsubstituted di(C1-C 18 Alkyl)amino, hydroxy substituted C1-C 18 Alkylamino or hydroxy substituted di(C1-C 18 Alkyl)amino, -O(CH2) y NR 15 R 16 or -O(CH2) y N + HR 15 R 16 An - 、-N(CH2) y NR 15 R 16, or -N(CH2) y N + HR 15 R 16 An - ,

[0121] in

[0122] An - It is the anion of a monovalent organic or inorganic acid;

[0123] y is an integer from 2 to 10;

[0124] R 15 is a saturated or unsaturated, linear or branched alkyl group having 1 to 22 carbon atoms;

[0125] R 16 is a saturated or unsaturated, linear or branched alkyl group having 1 to 22 carbon atoms;

[0126] Me + is a monovalent metal atom or an ammonium ion; and

[0127] Z is oxygen or sulfur.

[0128] The second step ii) is preferably an ester exchange reaction. In step ii), the alcohol is preferably of formula R c -[O-CH2-CH2-] c -OH ethoxylates, where R c is a saturated or unsaturated, linear or branched alkyl group having 1-22 carbon atoms, or an alkylaryl or dialkylaryl group having up to 24 carbon atoms, and c is 1-150.

[0129] Preferably, step i-1) or i-2) is carried out twice and a block copolymer is obtained, wherein in the first or second free radical polymerization step, the monomer or monomer mixture contains 50 to 100% by weight of C1-C6 alkyl ester of acrylic acid or methacrylic acid relative to the total monomers, and in the second or first free radical polymerization step, the ethylenically unsaturated monomer or monomer mixture contains at least one monomer without primary or secondary ester bonds.

[0130] In the first polymerization step, the monomer or monomer mixture contains 50 to 100 wt % of a C1-C6 alkyl ester of acrylic acid or methacrylic acid (first monomer) relative to the total monomers, and in the second polymerization step, the ethylenically unsaturated monomer or monomer mixture includes 4-vinyl-pyridine or pyridinium ion, 2-vinyl-pyridine or pyridinium ion, vinyl-imidazole or imidazolinium ion, 3-dimethylaminoethylacrylamide, 3-dimethylaminoethylmethacrylamide or the corresponding ammonium ion, 3-dimethylaminopropylacrylamide or the corresponding ammonium ion, or 3-dimethylaminopropylmethacrylamide or the corresponding ammonium ion (second monomer).

[0131] Preferably, the nitroxyl ether has the structure

[0132] The surface stabilizer is preferably a copolymer obtainable by a process comprising the steps of:

[0133] i-2) in a first step, in the presence of at least one nitroxyl ether having the following structural units,

[0134]

[0135] polymerizing a first monomer and a second monomer, wherein the first monomer is a C1-C6 alkyl or hydroxy C1-C6 alkyl acrylate or methacrylate, and the second monomer is selected from 4-vinyl-pyridine or pyridinium ion, 2-vinyl-pyridine or pyridinium ion, 1-vinyl-imidazole or imidazolinium ion, 3-dimethylaminoethylacrylamide, 3-dimethylaminoethylmethacrylamide, 3-dimethylamino-propylacrylamide, and 3-dimethylaminopropylmethacrylamide;

[0136] and ii) a second step, which comprises modifying the polymer or copolymer prepared in i-1) by transesterification, wherein the alcohol in step ii) is of formula R c -[O-CH2-CH2-] c -OH ethoxylates, where R c is a saturated or unsaturated, linear or branched alkyl group having 1-22 carbon atoms, or an alkylaryl or dialkylaryl group having up to 24 carbon atoms, and c is 1-150.

[0137] Preferably, the surface stabilizer obtained by the method described herein is a copolymer of the following formula (III):

[0138]

[0139] in

[0140] R 17a , R17b and R 17c are independently H or methyl;

[0141] R 18a and R 18b is H, or methyl;

[0142] R 19a is a saturated or unsaturated, linear or branched alkyl group having 1 to 22 carbon atoms;

[0143] R 19b For R c -[O-CH2-CH2-] c -O-;

[0144] R 19c for

[0145]

[0146] -C(=O)-NH-(CH2) y N + HR 15 R 16 An - ;

[0147] in

[0148] An - It is the anion of a monovalent organic or inorganic acid;

[0149] y is an integer from 2 to 10;

[0150] R 15 is a saturated or unsaturated, linear or branched alkyl group having 1 to 22 carbon atoms,

[0151] R 16 is a saturated or unsaturated, linear or branched alkyl group having 1 to 22 carbon atoms,

[0152] R c is a saturated or unsaturated, linear or branched alkyl group having 1-22 carbon atoms, or an alkylaryl or dialkylaryl group having up to 24 carbon atoms, and c is 1 to 150, and

[0153] y1, y2 and y3 are independently integers of 1 to 200. In the general formula (III), the sequence of the monomers with indices y1 and y2 may be fixed (block copolymers) or not (random copolymers).

[0154] Surface stabilizers of general formula (III) have been described in International Patent Application Publication No. WO200674969A1.

[0155] The preferred surface stabilizer of general formula (III) is a compound of general formula (III-a)

[0156]

[0157] in

[0158] R 18a and R 18b is H, or methyl;

[0159] y1, y2 and y3 are independently integers ranging from 1 to 200; and

[0160] c is an integer from 1 to 150. The sequence of the monomers with indices y1 and y2 may be fixed (block copolymers) or not (random copolymers).

[0161] Examples of preferred copolymers for use as surface stabilizers are the copolymers described in Example A3 and Example A6 of WO200674969A1.

[0162] In order to improve the stability of the optical properties of the silver nanosheets during storage or heat exposure, the silver nanosheets may be provided with a further surface stabilizer of the general formula (IV)

[0163]

[0164] in

[0165] R 9 A hydrogen atom or a -CHR 11 -N(R 12 )(R 13 )

[0166] R 10 is a hydrogen atom, a halogen atom, a C1-C8 alkoxy group, or a C1-C8 alkyl group;

[0167] R 11 is H, or C1-C8 alkyl; and

[0168] R 12 and R 13 are independently C1-C8 alkyl, hydroxy C1-C8 alkyl, or a group of the formula -[(CH2CH2)-O] n1 -CH2CH2-OH group, wherein n1 is 1-5.

[0169] Examples of compounds of formula (IV) include, but are not limited to:

[0170]

[0171] The dispersion of silver nanoflakes used to prepare the UV-Vis radiation curable security ink claimed herein can be obtained by using a method comprising the following steps:

[0172] 1) preparing a solution comprising a silver precursor and a compound of formula (II)

[0173]

[0174] in

[0175] R 1 H, C1-C 18 Alkyl, phenyl, C1-C8 alkylphenyl, or CH2COOH;

[0176] R 2 , R 3 , R 4 , R 5 , R 6 and R 7 are independently H, C1-C8 alkyl, or phenyl;

[0177] Y is O or NR 8 ;

[0178] R 8 is H, or C1-C8 alkyl;

[0179] k1 is an integer in the range of 1 to 500;

[0180] k2 and k3 are independently 0 or an integer in the range of 1 to 250;

[0181] k4 is 0 or 1; and

[0182] k5 is an integer ranging from 1 to 5;

[0183] The polymer or copolymer can be obtained by a process comprising the steps of:

[0184] i-1) In a first step, one or more ethylenically unsaturated monomers are polymerized in the presence of at least one nitroxyl ether having the following structural units:

[0185] wherein X represents a group having at least one carbon atom and such that a free radical X· originating from X is capable of initiating polymerization; or

[0186] i-2) In the first step, at least one stable nitroxyl radical and a free radical initiator, polymerizing one or more ethylenically unsaturated monomers; wherein at least one monomer used in step i-1) or i-2) is a C1-C6 alkyl or hydroxy C1-C6 alkyl ester of acrylic acid or methacrylic acid; and optionally

[0187] ii) a second step comprising modifying the polymer or copolymer prepared in i-1) or i-2) by transesterification, amidation, hydrolysis or anhydride modification or a combination thereof,

[0188] Water and optionally a defoamer;

[0189] 2) preparing a solution comprising a reducing agent and water, wherein the reducing agent comprises at least one boron atom in a molecule;

[0190] 3) adding the solution obtained in step 1) to the solution obtained in step 2), and adding one or more complexing agents;

[0191] 4) adding hydrogen peroxide solution to water; and

[0192] 5) Adding one or more surface stabilizers to the mixture obtained in step 4)

[0193] The silver precursor is a silver (I) compound selected from the group consisting of: AgNO3; AgClO4; Ag2SO4; AgCl; AgF; AgOH; Ag2O; AgBF4; AgIO3; AgPF6; R 200 CO2Ag、R 200 SO3Ag, where R 200 is unsubstituted or substituted C1-C 18 alkyl, unsubstituted or substituted C5-C8 cycloalkyl, unsubstituted or substituted C7-C 18 Arylalkyl, unsubstituted or substituted C6-C 18 Aryl or unsubstituted or substituted C2-C 18 heteroaryl; silver salts of dicarboxylic acids, tricarboxylic acids, polycarboxylic acids, polysulfonic acids, phosphoric acids and mixtures thereof, preferably selected from the group consisting of silver nitrate, silver acetate, silver perchlorate, silver methanesulfonate, silver benzenesulfonate, silver toluenesulfonate, silver trifluoromethanesulfonate, silver sulfate, silver fluoride and mixtures thereof, and more preferably silver nitrate.

[0194] The reducing agent is selected from the group consisting of alkali metal or alkaline earth metal borohydrides, such as sodium borohydride, alkali metal or alkaline earth metal acyloxy borohydrides, such as sodium triacetoxy borohydride, alkali metal or alkaline earth metal alkoxy or aryloxy borohydrides, such as sodium trimethoxy borohydride, aryloxy boranes, such as catechol borane, and amine-borane complexes, such as diethylaniline borane, tert-butylamine borane, morpholine borane, dimethylamine borane, triethylamine borane, pyridine borane, ammonia borane and mixtures thereof. Sodium borohydride is most preferred.

[0195] One or more complexing agents are selected from the group consisting of: chlorine-containing compounds that can release chloride ions under reaction conditions, such as metal chlorides, alkyl or aryl ammonium chlorides, phosphorus chlorides; primary or secondary amines and corresponding ammonium salts, such as methylamine or dimethylamine; ammonia and corresponding ammonium salts; and aminocarboxylic acids and their salts, such as ethylenediaminetetraacetic acid.

[0196] Non-limiting examples of complexing agents include ammonia, methylamine, dimethylamine, ethylamine, ethylenediamine, diethylenetriamine, ethylenediaminetetraacetic acid (EDTA); ethylenediamine N,N′-disuccinic acid (EDDS); methylglycine diacetic acid (MGDA); diethylenetriamine pentaacetic acid (DTPA); propylenediaminetetraacetic acid (PDTA); glutamic acid N,N-diacetic acid (N,N-dicarboxymethylglutamate tetrasodium salt (GLDA); nitrilotriacetic acid (NTA); and any salts thereof; N-hydroxyethylethylenediaminetriacetic acid (HEDTA), triethylenetetraaminehexaacetic acid (TTHA), N-hydroxyethyliminodiacetic acid (HEIDA), dihydroxyethylglycine (DHEG), ethylenediaminetetrapropionic acid (EDTP) and derivatives thereof, such as the trisodium salt of methylglycine diacetic acid (Na3MGDA) and the tetrasodium salt of EDTA.

[0197] Defoamers are compounds or compositions capable of inhibiting the formation of foam in the reaction mixture, for example, commercially available Foamex 1488, 1495, 3062, 7447, 800, 8030, 805, 8050, 810, 815N, 822, 825, 830, 835, 840, 842, 843, 845, 855, 860, 883, K 3, K 7, K 8, N, Antifoam SE-15 from Sigma, and Struktol SB-2080, etc. The amount of the defoaming agent is in the range of 0.00001% to 5% by weight, preferably 0.0001% to 3% by weight, and more preferably 0.001% to 2% by weight, relative to the total weight of the reaction mixture before adding hydrogen peroxide.

[0198] The defoaming agent may be added to the solution prepared in step 1) and / or to the solution prepared in step 2).

[0199] The reaction of silver nanosheet formation is carried out by gradually adding the silver precursor solution to the reducing agent solution, while the temperature of the two solutions is in the range of -3°C to 40°C, and the gradual addition is completed over a period of 15 minutes to 24 hours.

[0200] The silver nanosheets obtained in step 4) and / or 5) may be subjected to further purification and / or separation methods, such as decantation, (ultra)filtration, (ultra)centrifugation, reversible or irreversible coagulation, phase transfer with an organic solvent, and combinations thereof. The dispersion of silver nanosheets may contain up to about 99 wt-% silver nanosheets, preferably 5 wt-% to 99 wt-% silver nanosheets, more preferably 5 wt-% to 90 wt-% silver nanosheets, the wt-% being based on the total weight of the dispersion.

[0201] Starting from the silver nanosheets obtained by purification and / or separation, the silver nanosheets with the surface stabilizer of the general formula (I) can be prepared as follows:

[0202] i) In the presence of silver nanosheets, CS2 is reacted with a compound of formula R A R B The amine reaction of NH followed by R C R D NH treatment,

[0203] or

[0204] ii) By reacting CS2 with the formula R A R B The amine reaction of NH followed by R C R D NH treatment to obtain dithiocarbamate of general formula (I), which is then reacted with silver nanosheets.

[0205] With R A With R C Equal and R B With R D Equivalent silver nanosheets of dithiocarbamate of general formula (I) can be obtained starting from silver nanosheets that have been subjected to a purification and / or separation process:

[0206] iii) in the presence of silver nanosheets, CS2 is reacted with a compound of formula R A R B Amine reaction of NH; or

[0207] iv) by reacting CS2 with the formula R A R B NH amine reaction to obtain dithiocarbamate of general formula (I)

[0208]

[0209] Then react with silver nanosheets.

[0210] The silver nanoplatelets described herein are disclosed by European patent application No. 20206698.1, entitled “Compositions, comprising silver nanoplatelets”, filed by BASF SE on November 10, 2020.

[0211] The UV-Vis radiation curable security ink claimed herein comprises b) about 45 wt-% to about 80 wt-% of a cycloaliphatic epoxide, or a mixture of a cycloaliphatic epoxide and one or more UV-Vis radiation curable compounds. The one or more UV-Vis radiation curable compounds may include one or more cationic curable monomers, and / or one or more free radical curable monomers and / or oligomers. If the one or more UV-Vis radiation curable compounds include one or more free radical curable monomers and / or oligomers, the UV-Vis radiation curable security ink claimed herein further comprises g) one or more free radical photoinitiators. Therefore, the present invention relates to a UV-Vis radiation curable security ink for producing a security feature that appears blue when viewed under transmitted light and metallic yellow when viewed under incident light, wherein the ink comprises:

[0212] a) about 7.5 wt-% to about 20 wt-% of silver nanoflakes, the silver nanoflakes having an average diameter in the range of 50 to 150 nm with a standard deviation of less than 60%, an average thickness in the range of 5 to 30 nm with a standard deviation of less than 50%, and an average aspect ratio greater than 2.0, wherein the average diameter is determined by transmission electron microscopy, and the average thickness is determined by transmission electron microscopy, and wherein the silver nanoflakes have a surface stabilizer of formula (I)

[0213]

[0214] in

[0215] Residue R A is a C2-C4 alkyl group substituted with a hydroxyl group;

[0216] Residue R B is selected from C1-C4 alkyl, and C2-C4 alkyl substituted with hydroxyl; and

[0217] Cat + For the general formula + NH2R C R D The ammonium cation,

[0218] in

[0219] Residue R Cis a C2-C4 alkyl group substituted with a hydroxy group; and

[0220] Residue R D is selected from C1-C4 alkyl, and C2-C4 alkyl substituted with hydroxyl;

[0221] b) b-1) about 45 wt-% to about 80 wt-% of a cycloaliphatic epoxide;

[0222] b-2) a mixture of about 45 wt-% to about 80 wt-% of a cycloaliphatic epoxide and one or more cationic curable monomers;

[0223] b-3) a mixture of about 45 wt-% to about 80 wt-% of a cycloaliphatic epoxide and one or more free radical curable monomers and / or oligomers; or

[0224] b-4) a mixture of about 45 wt-% to about 80 wt-%, preferably about 45 wt-% to about 65 wt-%, of a cycloaliphatic epoxide, one or more cationic curable monomers and one or more free radical curable monomers and / or oligomers;

[0225] c) one or more cationic photoinitiators;

[0226] d) a perfluoropolyether surfactant functionalized with one or more functional groups selected from the group consisting of hydroxyl, acrylate, methacrylate, and trialkoxysilyl;

[0227] e) from about 3 wt-% to about 12 wt-% of a polyvinyl chloride copolymer, the polyvinyl chloride copolymer comprising at least 60 wt-% vinyl chloride; and optionally

[0228] f) up to about 25 wt-% of an organic solvent;

[0229] Provided that if the security ink comprises b-3) or b-4), the security ink further comprises g) one or more free radical photoinitiators; the weight percentages are based on the total weight of the UV-Vis radiation curable security ink.

[0230] A preferred embodiment according to the present invention relates to a UV-Vis radiation cationically curable security ink (i.e. an ink comprising only cationically curable monomers and no free radical curable monomers) for producing a security feature which appears blue when viewed under transmitted light and metallic yellow when viewed under incident light, wherein the ink comprises:

[0231] a) about 7.5 wt-% to about 20 wt-% of silver nanoflakes, the silver nanoflakes having an average diameter in the range of 50 to 150 nm with a standard deviation of less than 60%, an average thickness in the range of 5 to 30 nm with a standard deviation of less than 50%, and an average aspect ratio greater than 2.0, wherein the average diameter is determined by transmission electron microscopy, and the average thickness is determined by transmission electron microscopy, and wherein the silver nanoflakes have a surface stabilizer of formula (I)

[0232]

[0233] in

[0234] Residue R A is a C2-C4 alkyl group substituted with a hydroxyl group;

[0235] Residue R B is selected from C1-C4 alkyl, and C2-C4 alkyl substituted with hydroxyl; and

[0236] Cat + For the general formula + NH2R C R D of ammonium cations, where

[0237] Residue R C is a C2-C4 alkyl group substituted with a hydroxy group; and

[0238] Residue R D is selected from C1-C4 alkyl, and C2-C4 alkyl substituted with hydroxyl;

[0239] b) b-1) about 45 wt-% to about 80 wt-% of a cycloaliphatic epoxide; or

[0240] b-2) a mixture of about 45 wt-% to about 80 wt-% of a cycloaliphatic epoxide and one or more cationic curable monomers;

[0241] c) one or more cationic photoinitiators;

[0242] d) a perfluoropolyether surfactant functionalized with one or more functional groups selected from the group consisting of hydroxyl, acrylate, methacrylate, and trialkoxysilyl;

[0243] e) from about 3 wt-% to about 12 wt-% of a polyvinyl chloride copolymer, the polyvinyl chloride copolymer comprising at least 60 wt-% vinyl chloride; and optionally

[0244] f) up to about 25 wt-% of an organic solvent; the weight percentages are based on the total weight of the UV-Vis radiation cationically curable safety ink. If the UV-Vis radiation cationically curable safety ink comprises b-2) about 45 wt-% to about 80 wt-% of a cycloaliphatic epoxide and a mixture of one or more cationic curable monomers, it is preferred that the ratio between the weight percentage (wt-%) of the one or more cationic curable monomers and the weight percentage (wt-%) of the cycloaliphatic epoxide is less than 1.4:1, preferably less than 1:1, and more preferably less than 0.9:1.

[0245] One alternative preferred embodiment according to the present invention relates to a UV-Vis radiation curable hybrid security ink (i.e. an ink comprising both cationically curable monomers and free radically curable monomers / oligomers) for producing a security feature that appears blue when viewed in transmitted light and metallic yellow when viewed in incident light, wherein the ink comprises:

[0246] a) about 7.5 wt-% to about 20 wt-% of silver nanoflakes, the silver nanoflakes having an average diameter in the range of 50 to 150 nm with a standard deviation of less than 60%, an average thickness in the range of 5 to 30 nm with a standard deviation of less than 50%, and an average aspect ratio greater than 2.0, wherein the average diameter is determined by transmission electron microscopy, and the average thickness is determined by transmission electron microscopy, and wherein the silver nanoflakes have a surface stabilizer of formula (I)

[0247]

[0248] in

[0249] Residue R A is a C2-C4 alkyl group substituted with a hydroxyl group;

[0250] Residue R B is selected from C1-C4 alkyl, and C2-C4 alkyl substituted with hydroxyl; and

[0251] Cat + For the general formula + NH2R C R D The ammonium cation,

[0252] The residue R C is a C2-C4 alkyl group substituted with a hydroxy group; and

[0253] Residue R D is selected from C1-C4 alkyl, and C2-C4 alkyl substituted with hydroxyl;

[0254] b) b-3) a mixture of about 45 wt-% to about 80 wt-% of a cycloaliphatic epoxide and one or more free radical curable monomers and / or oligomers; or

[0255] b-4) a mixture of about 45 wt-% to about 80 wt-%, preferably about 45 wt-% to about 65 wt-%, of a cycloaliphatic epoxide, one or more cationic curable monomers and one or more free radical curable monomers and / or oligomers;

[0256] c) one or more cationic photoinitiators;

[0257] d) a perfluoropolyether surfactant functionalized with one or more functional groups selected from the group consisting of hydroxyl, acrylate, methacrylate, and trialkoxysilyl;

[0258] e) from about 3 wt-% to about 12 wt-% of a polyvinyl chloride copolymer comprising at least 60 wt-% vinyl chloride; and optionally;

[0259] g) one or more free radical photoinitiators; and optionally

[0260] f) up to about 25 wt-% of an organic solvent;

[0261] The weight percentages are based on the total weight of the UV-Vis radiation hybrid curable safety ink. If the hybrid ink claimed herein contains b-3) a mixture of about 45 wt-% to about 80 wt-% of a cycloaliphatic epoxide and one or more free radical curable monomers and / or oligomers, the ratio between the total weight percentage (wt-%) of the one or more free radical curable monomers and / or oligomers and the weight percentage (wt-%) of the cycloaliphatic epoxide is preferably lower than 1.6:1, more preferably lower than 1:1, and even more preferably lower than 0.5:1. If the mixed ink claimed herein contains b-4) a mixture of about 45 wt-% to about 80 wt-% of a cycloaliphatic epoxide, one or more cationic curable monomers and one or more free radical curable monomers and / or oligomers, the ratio between the total weight percentage (wt-%) of the one or more free radical curable monomers and / or oligomers and the sum of the weight percentage (wt-%) of the cycloaliphatic epoxide and the total weight percentage (wt-%) of the one or more cationic curable monomers is preferably less than 1.6:1, more preferably less than 1:1, and even more preferably less than 0.5:1, and the ratio between the weight percentage (wt-%) of the one or more cationic curable monomers and the weight percentage (wt-%) of the cycloaliphatic epoxide is preferably less than 1.4:1, more preferably less than 1:1, and even more preferably less than 0.9:1.

[0262] Advantageously, the UV-Vis radiation cationically curable security inks claimed herein and the UV-Vis radiation hybrid curable security inks claimed herein provide security features with improved mechanical resistance properties compared to security features known in the art obtained from UV radical curable inks or solvent-based inks, in particular from UV radical curable inks or solvent-based inks containing a high concentration of silver nanoflakes.

[0263] As is well known to those skilled in the art, cycloaliphatic epoxides are cationically curable monomers containing at least one substituted or unsubstituted epoxycyclohexyl residue.

[0264]

[0265] Preferably, the alicyclic epoxide described herein comprises at least one cyclohexane ring and at least two epoxy groups. More preferably, the alicyclic epoxide is a compound of formula (V):

[0266]

[0267] Wherein -L- represents a single bond or a divalent group containing one or more atoms. The alicyclic epoxide of general formula (V) is optionally substituted by one or more linear or branched alkyl groups containing 1 to 10 carbon atoms (such as methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, sec-butyl, tert-butyl, hexyl, octyl, and decyl), and preferably a linear or branched alkyl group containing 1 to 3 carbon atoms (such as methyl, ethyl, n-propyl, and isopropyl).

[0268] In the general formula (V), the divalent group -L- may be a linear or branched alkylene group containing 1 to 18 carbon atoms. Examples of the linear or branched alkylene group include, but are not limited to, methylene, methylmethylene, dimethylmethylene, ethylene, propylene, and trimethylene.

[0269] In the general formula (V), the divalent group -L- may be a divalent alicyclic hydrocarbon group or a cycloalkylene group, such as 1,2-cyclopentylene, 1,3-cyclopentylene, cyclopentylene, 1,2-cyclohexylene, 1,3-cyclohexylene, 1,4-cyclohexylene, and cyclohexylene.

[0270] In the general formula (V), -L- can be a divalent group containing one or more oxygen-containing linking groups, wherein the oxygen-containing linking groups are selected from the group consisting of -C(═O)-, -OC(═O)O-, -C(═O)O-, and -O-. Preferably, the alicyclic epoxide is an alicyclic epoxide of the general formula (V), wherein -L- is a divalent group containing one or more oxygen-containing linking groups, wherein the oxygen-containing linking groups are selected from the group consisting of -C(═O)-, -OC(═O)O-, -C(═O)O-, and -O-, and more preferably an alicyclic epoxide of the general formula (Va), (Vb), or (Vc) defined below:

[0271]

[0272] in

[0273] L 1 may be the same or different at each occurrence and is a straight chain or branched chain alkyl group containing 1 to 10 carbon atoms (such as methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, sec-butyl, tert-butyl, hexyl, octyl, and decyl), and preferably a straight chain or branched chain alkyl group containing 1 to 3 carbon atoms (such as methyl, ethyl, n-propyl, and isopropyl);

[0274] L 2 may be the same or different at each occurrence and is a straight chain or branched chain alkyl group containing 1 to 10 carbon atoms (such as methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, sec-butyl, tert-butyl, hexyl, octyl, and decyl), and preferably a straight chain or branched chain alkyl group containing 1 to 3 carbon atoms (such as methyl, ethyl, n-propyl, and isopropyl); and

[0275] l1 and l2 are independently an integer between 0 and 9, preferably an integer between 0 and 3;

[0276]

[0277] in

[0278] L 1 may be the same or different at each occurrence and is a straight chain or branched chain alkyl group containing 1 to 10 carbon atoms (such as methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, sec-butyl, tert-butyl, hexyl, octyl, and decyl), and preferably a straight chain or branched chain alkyl group containing 1 to 3 carbon atoms (such as methyl, ethyl, n-propyl, and isopropyl);

[0279] L 2may be the same or different at each occurrence and is a straight chain or branched chain alkyl group containing 1 to 10 carbon atoms (such as methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, sec-butyl, tert-butyl, hexyl, octyl, and decyl), and preferably a straight chain or branched chain alkyl group containing 1 to 3 carbon atoms (such as methyl, ethyl, n-propyl, and isopropyl); and

[0280] l1 and l2 are independently an integer between 0 and 9, preferably an integer between 0 and 3;

[0281] –L 3 - is a single bond or a straight or branched divalent hydrocarbon group containing 1 to 10 carbon atoms, and preferably containing 3 to 8 carbon atoms, such as an alkylene group including trimethylene, tetramethylene, hexamethylene and 2-ethylhexylene, and a cycloalkylene group such as 1,2-cyclohexylene, 1,3-cyclohexylene and 1,4-cyclohexylene, and cyclohexylene;

[0282]

[0283] in

[0284] L 1 may be the same or different at each occurrence and is a straight or branched chain alkyl group containing 1 to 3 carbon atoms, such as methyl, ethyl, n-propyl, and isopropyl;

[0285] L 2 may be the same or different at each occurrence and is a straight or branched chain alkyl group containing 1 to 3 carbon atoms, such as methyl, ethyl, n-propyl, and isopropyl; and

[0286] l1 and l2 are independently an integer between 0 and 9, preferably an integer between 0 and 3.

[0287] Preferred alicyclic epoxides of general formula (Va) include, but are not limited to, 3,4-epoxycyclohexylmethyl-3,4-epoxycyclohexanecarboxylate, 3,4-epoxy-6-methyl-cyclohexylmethyl-3,4-epoxy-6-methylcyclohexanecarboxylate, 3,4-epoxy-2-methyl-cyclohexylmethyl-3,4-epoxy-2-methyl-cyclohexanecarboxylate, and 3,4-epoxy-4-methyl-cyclohexylmethyl-3,4-epoxy-4-methylcyclohexanecarboxylate.

[0288] Preferred alicyclic epoxides of general formula (Vb) include, but are not limited to, bis(3,4-epoxycyclohexylmethyl)adipate, bis(3,4-epoxy-6-methylcyclohexylmethyl)adipate, bis(3,4-epoxycyclohexylmethyl)oxalate, bis(3,4-epoxycyclohexylmethyl)pimelate, and bis(3,4-epoxycyclohexylmethyl)sebacate.

[0289] A preferred cycloaliphatic epoxide of the general formula (Vc) is 2-(3,4-epoxycyclohexyl-5,5-spiro-3,4-epoxy)cyclohexane-m-dioxane.

[0290] Other alicyclic epoxides include alicyclic epoxides of the general formula (VI-a) and alicyclic epoxides of the general formula (VI-b), which are optionally substituted with one or more straight-chain or branched alkyl groups containing 1 to 10 carbon atoms (such as methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, sec-butyl, tert-butyl, hexyl, octyl, and decyl), and preferably with a straight-chain or branched alkyl group containing 1 to 3 carbon atoms (such as methyl, ethyl, n-propyl, and isopropyl).

[0291]

[0292] The cycloaliphatic epoxides described herein may be hydroxy-modified or (meth)acrylate-modified. Examples are commercially available from Daicel Corp. under the names Cyclomer A400 (CAS: 64630-63-3) and Cyclomer M100 (CAS: 82428-30-6), or from TetraChem / Jiangsu under TTA 15 and TTA 16 46.

[0293] The one or more cationic curable monomers described herein are selected from the group consisting of: vinyl ethers, propenyl ethers, cyclic ethers other than alicyclic epoxides, lactones, cyclic thioethers, vinyl thioethers, propenyl thioethers, hydroxyl-containing compounds, and mixtures thereof, preferably selected from the group consisting of: vinyl ethers, cyclic ethers other than alicyclic epoxides, and mixtures thereof. Cyclic ethers other than alicyclic epoxides include epoxides other than alicyclic epoxides, oxetanes, and tetrahydrofuran. Preferably, the ratio between the total weight percentage (wt-%) of the one or more cationic curable monomers and the weight percentage (wt-%) of the alicyclic epoxide is less than 1.4:1, more preferably less than 1:1, most preferably less than 0.9:1, and particularly preferably less than 0.8:1.

[0294] Vinyl ethers are known in the art and promote curing and reduce viscosity, thus limiting the risk of sticking and set-off when the printed sheets are placed in a pile immediately after printing and curing. They also improve the physical and chemical resistance of the printed security elements and increase the flexibility of the printed and cured ink layer and its adhesion to the substrate, which is particularly advantageous for printing on plastic and polymer substrates. Vinyl ethers also help to reduce the viscosity of the ink, while strongly copolymerizing with the ink vehicle. Examples of preferred vinyl ethers for use in the security inks claimed herein include methyl vinyl ether, ethyl vinyl ether, n-propyl vinyl ether, n-butyl vinyl ether, isobutyl vinyl ether, ethylhexyl vinyl ether, octadecyl vinyl ether, dodecyl vinyl ether, isopropyl vinyl ether, tert-butyl vinyl ether, tert-amyl vinyl ether, cyclohexyl vinyl ether, cyclohexanedimethanol monovinyl ether, cyclohexanedimethanol divinyl ether, 4-(vinyloxymethyl)cyclohexylmethylbenzoate, phenyl vinyl ether, methylphenyl vinyl ether, methoxyphenyl vinyl ether, 2-chloroethyl vinyl ether, 2-hydroxyethyl vinyl ether, 4-hydroxybutyl vinyl ether, 1,6-hexanediol monovinyl ether, ethylene glycol divinyl ether, ethylene glycol monovinyl ether, 1,4-butanediol divinyl ether, 1,6-hexanediol divinyl ether, 4-(vinyloxy)butylbenzoate, bis[4-(vinyloxy)butyl]hexanediol divinyl ether, bis[4-(vinyloxy)butyl]succinate, bis[4-(vinyloxymethyl)cyclohexylmethyl]glutarate, 4-(vinyloxy)butyl stearate, trimethylolpropane trivinyl ether, propenyl ether of propylene carbonate, diethylene glycol monovinyl ether, diethylene glycol divinyl ether, ethylene glycol butyl vinyl ether, dipropylene glycol divinyl ether, triethylene glycol divinyl ether, triethylene glycol methyl vinyl ether, triethylene glycol monobutyl ether, tetraethylene glycol divinyl ether , poly(tetrahydrofuran) divinyl ether, polyethylene glycol-520 methyl vinyl ether, pluriol-E200 divinyl ether, tris[4-(vinyloxy)butyl]trimellitate, 1,4-bis(2-vinyloxyethoxy)benzene, 2,2-bis(4-vinyloxyethoxyphenyl)propane, bis[4-(vinyloxy)methyl]cyclohexyl]methyl]terephthalate, bis[4-(vinyloxy)methyl]cyclohexyl]methyl]isophthalate. Suitable vinyl ethers are commercially available from BASF under the names EVE, IBVE, DDVE, ODVE, BDDVE, DVE-2, DVE-3, CHVE, CHDM-di, HBVE. One or more of the vinyl ethers described herein may be hydroxy-modified or (meth)acrylate-modified (e.g. VEEA, 2-(2-vinyloxyethoxy)ethyl acrylate (CAS: 86273-46-3) from Nippon Shokubai).

[0295] Oxetanes are known in the art and accelerate curing and reduce tack, thus limiting the risk of sticking and offsetting when the printed sheets are placed in a pile immediately after printing and curing. They also help to reduce the viscosity of the ink, while strongly copolymerizing with the ink vehicle. Preferred examples of oxetanes include trimethyleneoxide, 3,3-dimethyloxetane, trimethylolpropaneoxetane, 3-ethyl-3-hydroxymethyloxetane, 3-ethyl-3-[(2-ethylhexyloxy)methyl]oxetane, 3,3-dicyclomethyloxetane, 3-ethyl-3-phenoxymethyloxetane, bis([1-ethyl(3-oxetanyl)]methyl)ether, 1,4-bis[3-ethyl-3-oxetanylmethoxy)methyl]benzene, 3,3-dimethyl-2(p-methoxy-phenyl)-oxetane, 3-ethyl-[(tri-ethoxysilylpropoxy)methyl]oxetane, 4,4-bis(3-ethyl-3-oxetanyl)methoxymethyl]biphenyl and 3,3-dimethyl-2(p-methoxy-phenyl)oxetane. The one or more oxetanes described herein may be hydroxy-modified or (meth)acrylate-modified (eg, UVi-Cure S170 from Lambson (CAS: 37674-57-0)).

[0296] The use of epoxides in UV-VIS radiation curable inks helps accelerate curing and reduce viscosity, as well as helps reduce the viscosity of the ink, while strongly copolymerizing with the ink vehicle. Preferred examples of epoxides other than the alicyclic epoxides described herein include, but are not limited to, cyclohexanedimethanol diglycidyl ether, poly(ethylene glycol) diglycidyl ether, poly(propylene glycol) diglycidyl ether, butanediol diglycidyl ether, hexanediol diglycidyl ether, bisphenol A diglycidyl ether, neopentyl glycol diglycidyl ether, trimethylolpropane triglycidyl ether, glycerol triglycidyl ether, pentaerythritol tetraglycidyl ether, butyl glycidyl ether, p-tert-butylphenyl glycidyl ether, hexadecyl glycidyl ether, 2-ethyl-hexyl glycidyl ether, octyl glycidyl ether, decyl glycidyl ether, dodecyl glycidyl ether, tetradecyl glycidyl ether, C 12 / C 14 -Alkyl glycidyl ether, C 13 / C 15 - alkyl glycidyl ethers and mixtures thereof. Suitable epoxides other than cycloaliphatic epoxides are manufactured by EMS Griltech under the trademark (For example, V51-63 or RV 1806) are commercially available.

[0297] The free radical curable monomer described herein is selected from the group consisting of mono(meth)acrylates, di(meth)acrylates, tri(meth)acrylates, tetra(meth)acrylates, and mixtures thereof, preferably selected from the group consisting of tri(meth)acrylates, tetra(meth)acrylates, and mixtures thereof. The term "(meth)acrylate" in the context of the present invention refers to acrylates and corresponding methacrylates.

[0298] Preferred examples of the mono(meth)acrylates include 2(2-ethoxyethoxy)ethyl(meth)acrylate, 2-phenoxyethyl(meth)acrylate, C(meth)acrylate, 12 / C 14 Alkyl esters, (meth) acrylic acid C 16 / C 18 Alkyl esters, caprolactone (meth)acrylate, cyclic trimethylolpropane formal (meth)acrylate, nonylphenol (meth)acrylate, isobornyl (meth)acrylate, isodecyl (meth)acrylate, lauryl (meth)acrylate, stearyl (meth)acrylate, octyldecyl (meth)acrylate, tridecyl (meth)acrylate, methoxy poly (ethylene glycol) (meth)acrylate, polypropylene glycol (meth)acrylate, tetrahydrofurfuryl (meth)acrylate, 1,3-butanediol di (meth)acrylate, 1,4-butanediol di (meth)acrylate, 1,6-hexanediol di (meth)acrylate, 3-methyl-1,5-pentanediol di (meth)acrylate, alkoxylated di (meth)acrylates, ester diol di (meth)acrylates, and mixtures thereof.

[0299] Preferred examples of di(meth)acrylates include bisphenol A di(meth)acrylates, alkoxylated (e.g., ethoxylated and propoxylated) bisphenol A di(meth)acrylates, bisphenol A diglycidyl ether di(meth)acrylate, ethylene glycol di(meth)acrylate, diethylene glycol di(meth)acrylate, triethylene glycol di(meth)acrylate, tetraethylene glycol di(meth)acrylate, dipropylene glycol di(meth)acrylate, tripropylene glycol di(meth)acrylate, polyethylene glycol di(meth)acrylate, neopentyl glycol di(meth)acrylate, tricyclodecane dimethanol di(meth)acrylate, and mixtures thereof.

[0300] Preferred examples of tri(meth)acrylates include trimethylolpropane tri(meth)acrylates, alkoxylated (e.g., ethoxylated and propoxylated) trimethylolpropane tri(meth)acrylates, alkoxylated (e.g., ethoxylated and propoxylated) glycerol tri(meth)acrylates, pentaerythritol tri(meth)acrylates, alkoxylated pentaerythritol tri(meth)acrylates, alkoxylated (e.g., ethoxylated and propoxylated) pentaerythritol tri(meth)acrylates, and mixtures thereof.

[0301] Preferred examples of tetra(meth)acrylates include di(trimethylolpropane) tetra(meth)acrylates, pentaerythritol tetra(meth)acrylates, alkoxylated (e.g., ethoxylated and propoxylated) pentaerythritol tetra(meth)acrylates, and mixtures thereof, preferably selected from the group consisting of di(trimethylolpropane) tetra(meth)acrylates, alkoxylated pentaerythritol tetra(meth)acrylates, and mixtures thereof.

[0302] As used herein, the term "free radical curable oligomer" refers to a free radical curable (meth)acrylate oligomer, which may be branched or substantially linear, and may have terminal and / or pendant (meth)acrylate functional groups. Preferably, the free radical curable oligomer is selected from the group consisting of (meth)acrylic oligomers, polyurethane (meth)acrylate oligomers, polyester (meth)acrylate oligomers, polyether (meth)acrylate oligomers, epoxy (meth)acrylate oligomers, and mixtures thereof, more preferably selected from the group consisting of polyester (meth)acrylate oligomers, epoxy (meth)acrylate oligomers, and mixtures thereof.

[0303] Suitable examples of epoxy (meth) acrylate oligomers include, but are not limited to, aliphatic epoxy (meth) acrylate oligomers, particularly mono (meth) acrylates, di (meth) acrylates and tri (meth) acrylates, and aromatic epoxy (meth) acrylate oligomers. Suitable examples of aromatic epoxy (meth) acrylate oligomers include bisphenol A (meth) acrylate oligomers such as bisphenol A mono (meth) acrylates, bisphenol A di (meth) acrylates and bisphenol A tri (meth) acrylates, and alkoxylated (e.g., ethoxylated and propoxylated) bisphenol A (meth) acrylate oligomers such as alkoxylated bisphenol A mono (meth) acrylates, alkoxylated bisphenol A di (meth) acrylates and alkoxylated bisphenol A tri (meth) acrylates, preferably ethoxylated bisphenol A di (meth) acrylates.

[0304] The security ink claimed herein comprises c) one or more cationic photoinitiators. Preferably, the amount of the one or more cationic photoinitiators in the UV-Vis radiation cationically curable security ink claimed herein (i.e., an ink comprising only cationically curable monomers and no free radical curable monomers) is from about 1 wt-% to about 10 wt-%, preferably from about 1.1 wt-% to about 8 wt-%, more preferably from about 1.1 wt-% to about 6 wt-%, wherein the weight percentages are based on the total weight of the UV-Vis radiation cationically curable ink. Preferably, the amount of the one or more cationic photoinitiators in the UV-Vis radiation hybrid curable security ink claimed herein (i.e., an ink comprising both cationically curable monomers and free radical curable monomers) is from 1 wt-% to about 6 wt-%, wherein the weight percentages are based on the total weight of the UV-Vis radiation cationically curable ink.

[0305] One or more cationic photoinitiators described herein (also referred to as photo-acid generators in the art) are onium salts, preferably selected from the group consisting of azonium salts, oxonium salts, iodonium salts, sulfonium salts and mixtures thereof, more preferably selected from the group consisting of oxonium salts, iodonium salts, sulfonium salts and mixtures thereof, and even more preferably selected from the group consisting of sulfonium salts, iodonium salts, and mixtures thereof.

[0306] The iodonium salt described herein has a cation part and an anion part, wherein the anion part is preferably BF4 - 、B(C6F5)4 - PF6 - 、AsF6 - 、SbF6 - or CF3SO3 - , more preferably SbF6 -, and wherein the cationic moiety is preferably an aromatic iodonium ion, more preferably an iodonium ion containing two aromatic groups, wherein the two aromatic groups may be independently substituted by one or more alkyl groups (e.g., methyl, ethyl, isobutyl, tert-butyl, etc.), one or more alkoxy groups, one or more nitro groups, one or more halogen-containing groups, one or more hydroxyl groups, or a combination thereof, preferably substituted by one or more alkyl groups. Particularly suitable iodonium salts of the present invention are commercially available from DEUTERON under the names DEUTERON UV 1240, DEUTERON UV 1242, DEUTERON UV 2257, DEUTERON UV 1250, and DEUTERON UV 3100, commercially available from IGM Resins under the names OMNICAT 250, OMNICAT 440, and OMNICAT 445, commercially available from Lambson under the names SpeedCure 937, SpeedCure 938, and SpeedCure 939.

[0307] The sulfonium salt described herein has a cation part and an anion part, wherein the anion part is preferably BF4 - 、B(C6F5)4 - PF6 - ,(PF 6-h (C j F 2j-1 ) h ) - (wherein h is an integer from 1 to 5, and j is an integer from 1 to 4), AsF6 - 、SbF6 - CF3SO3 - , perfluoroalkyl sulfonate or pentafluorohydroxy antimonate, more preferably SbF6 -, and the cationic part is preferably an aromatic sulfonium salt, more preferably a sulfonium ion containing two or more aryl groups, wherein the two or more aryl groups can be independently substituted by one or more alkyl groups (e.g., methyl, ethyl, isobutyl, tert-butyl, etc.), one or more alkoxy groups, one or more aryloxy groups, one or more halogen-containing groups, one or more hydroxyl groups, or a combination thereof. Suitable examples of sulfonium ions containing two or more aryl groups include, but are not limited to, triarylsulfonium ions, diphenyl[4-(phenylthio)phenyl]sulfonium ions, bis[4-(diphenylsulfonium)phenyl]sulfonium ions, triphenylsulfonium ions, and tris[4-(4-acetylphenyl)sulfanylphenyl]sulfonium ions. Particularly suitable examples of sulfonium salts of the present invention are those commercially available under the names SpeedCure 976, SpeedCure 976D, SpeedCure 976S and SpeedCure 992, all from Lambson, ESACURE 1187, OMNICAT 270, OMNICAT 320, OMNICAT 432 and OMNICAT 550, all from IGM Resins, and DoubleCure 1176, DoubleCure 1190 and DoubleCure 1172, all from DoubleBond.

[0308] The oxonium salt described herein has a cation part and an anion part, wherein the anion part is preferably BF4 - 、B(C6F5)4 - PF6 - 、AsF6 - 、SbF6 - or CF3SO3 - , more preferably BF4 - , and the cationic part is preferably an aromatic oxonium ion, more preferably a pyrylium ion, which is preferably substituted by one or more aryl groups, wherein one or more aryl groups can be independently substituted by one or more alkyl groups (e.g., methyl, ethyl, isobutyl, tert-butyl, etc.), one or more alkoxy groups, one or more nitro groups, one or more halogen groups, one or more hydroxyl groups or a combination thereof. A particularly suitable oxonium salt of the present invention is 2,4,6-triphenylpyrylium tetrafluoroborate.

[0309] Further examples of useful cationic photoinitiators can be found in standard textbooks such as "Chemistry & Technology of UV & EB Formulation for Coatings, Inks & Paints", Volume III, "Photoinitiators for Free Radical Cationic and Anionic Polymerization", 2nd Edition, JV Crivello & K. Dietliker, edited by G. Bradley and published in 1998 by John Wiley & Sons in association with SITA Technology Limited.

[0310] In addition, the hybrid security ink claimed herein comprises g) one or more free radical photoinitiators. Preferably, the amount of the one or more free radical photoinitiators in the UV-Vis radiation hybrid curable ink described herein is about 1 wt-% to about 6 wt-%, the weight percentage being based on the total weight of the UV-Vis radiation hybrid curable ink.

[0311] As used herein, the one or more free radical photoinitiators are preferably selected from the group consisting of hydroxyketones (e.g., α-hydroxyketones), alkoxyketones (e.g., α-alkoxyketones), acetophenones, benzophenones, ketosulfones, benzyl ketals, benzoin ethers, phosphine oxides, phenylglyoxylates, thioxanthones, and mixtures thereof, more preferably selected from the group consisting of phosphine oxides, hydroxyketones, thioxanthones, and mixtures thereof.

[0312] Suitable α-hydroxyketones include, without limitation, (1-[4-(2-hydroxyethoxy)-phenyl]-2-hydroxy-2-methyl-1-propan-1-one), 1-hydroxycyclohexyl phenyl ketone, 2-hydroxy-2-methyl-1-phenylpropan-1-one, 2-hydroxy-2-methyl-1-(4-tert-butyl)phenylpropan-1-one, 2-hydroxy-1-[4-[[4-(2-hydroxy-2-methylpropionyl)phenyl]methyl]phenyl]-2-methylpropan-1-one, 2-hydroxy-1-[4-[4-(2-hydroxy-2-methylpropionyl)phenoxy]phenyl]-2-methylpropan-1-one, and oligo[2-hydroxy-2-methyl-1-[4-(1-methylvinyl)phenyl]propanone].

[0313] Suitable acetophenones include, without limitation, 2,2-diethoxyacetophenone and 2-methoxy-2-phenylacetophenone.

[0314] Suitable benzophenones include, but are not limited to, benzophenone, polymeric benzophenone derivatives, 2-methylbenzophenone, 3-methylbenzophenone, 4-methylbenzophenone, 2,4,6-trimethylbenzophenone, 3,3′-dimethyl-4-methoxybenzophenone, 4-phenylbenzophenone, 4-chlorobenzophenone, methyl-2-benzoylbenzoate, 4-(4-methylphenylthio)benzophenone, 4-hydroxybenzophenone laurate, and a mixture of 50% benzophenone and 50% 1-hydroxycyclohexyl phenyl ketone.

[0315] Suitable ketosulfones include, without limitation, 1-[4-(4-benzoylphenylsulfanyl)phenyl]-2-methyl-2-(4-methylphenylsulfonyl)propan-1-one.

[0316] Suitable benzyl ketals include, without limitation, 2,2-dimethoxy-2-phenylacetophenone.

[0317] Suitable benzoin ethers include, without limitation, 2-ethoxy-1,2-diphenylethanone, 2-isopropoxy-1,2-diphenylethanone, 2-isobutoxy-1,2-diphenylethanone, 2-butoxy-1,2-diphenylethanone, 2,2-dimethoxy-1,2-diphenylethanone, and 2,2-diethoxyacetophenone.

[0318] Suitable phosphine oxides include, but are not limited to, 2,4,6-trimethylbenzoyldiphenylphosphine oxide, ethyl phenyl(2,4,6-trimethylbenzoyl)phenylphosphine oxide, phenylbis(2,4,6-trimethylbenzoyl)phosphine oxide, bis(2,6-dimethoxybenzoyl)-2,4,4-trimethylpentylphosphine oxide, substituted acyl-phosphine oxides, mixtures of diphenyl(2,4,6-trimethylbenzoyl)phosphine oxide and 2-hydroxy-2-methylpropiophenone, mixtures of phenylbis(2,4,6-trimethylbenzoyl)phosphine oxide and 2-hydroxy-2-methylpropiophenone, mixtures of ethyl(2,4,6-trimethylbenzoyl)phenylphosphine oxide and 2-hydroxy-2-methylpropiophenone, and mixtures of phenylbis(2,4,6-trimethylbenzoyl)phosphine oxide and ethyl phenyl(2,4,6-trimethylbenzoyl)phenylphosphine oxide.

[0319] Suitable thioxanthones include, without limitation, 2-methylthioxanthone, 2,4-diethylthioxanthone, 2-isopropylthioxanthone, 1-chloro-4-propoxythioxanthone, and polymeric thioxanthone derivatives.

[0320] Suitable phenylglyoxylic acid esters include, but are not limited to, methyl benzoylformate, 2-[2-oxo-2-phenyl-acetoxy-ethoxy]ethyl 2-oxo-2-phenylacetate, and a mixture of 2-[2-oxo-2-phenyl-acetoxy-ethoxy]ethyl 2-oxo-2-phenylacetate and oxy-phenyl-acetic acid 2-[2-hydroxy-ethoxy]-ethyl ester.

[0321] Preferably, the one or more free radical photoinitiators are phosphine oxides as described herein, and more preferably a mixture of phenylbis(2,4,6-trimethylbenzoyl)phosphine oxide and ethyl phenyl(2,4,6-trimethylbenzoyl)phenylphosphonate.

[0322] The UV-Vis radiation curable security ink described herein comprises d) a perfluoropolyether surfactant functionalized with one or more, preferably two or more, functional groups selected from the group consisting of hydroxyl, acrylate, methacrylate, and trialkoxysilyl. Surprisingly, it has been found that the use of a perfluoropolyether functionalized with one or more, preferably two or less, functional groups selected from the group consisting of hydroxyl, acrylate, methacrylate, and trialkoxysilyl as a surfactant in the UV-Vis radiation curable ink described herein is essential for producing a security feature that exhibits a metallic yellow color when viewed under incident light. As demonstrated in Tables 3c and 4c, UV-Vis radiation curable inks comprising only a perfluoropolyether surfactant functionalized with one or more functional groups selected from the group consisting of hydroxyl, acrylate, methacrylate, and trialkoxysilyl provide a security feature that exhibits a metallic yellow color when viewed under incident light. Security features produced with UV-Vis radiation curable inks lacking surfactants (e.g., Ink C8), or UV-Vis radiation curable inks containing perfluoropolyether surfactants lacking functional groups (e.g., Ink C1), or UV-Vis radiation curable inks lacking surfactants with a perfluoropolyether backbone (e.g., Inks C2–C7) appear brown to dark brown in reflection, which is not noticeable to the layman and, therefore, is not suitable as a dichroic security feature for protecting valuable documents.

[0323] The perfluoropolyether surfactant functionalized with one or more functional groups selected from the group consisting of hydroxyl, acrylate, methacrylate, and trialkoxysilyl comprises a perfluoropolyether backbone and one or more, preferably two or more terminal functional groups selected from the group consisting of hydroxyl, acrylate, methacrylate, and trialkoxysilyl, the perfluoropolyether surfactant being characterized in that the average molecular weight (Mn) is less than about 2000 [g / mol]. As used herein, the perfluoropolyether backbone refers to the residue of a perfluoropolyether polymer comprising randomly distributed repeating units selected from perfluoromethyleneoxy (—CF2O—) and perfluoroethyleneoxy (—CF2-CF2O—). The perfluoropolyether residue is directly or through a spacer connected to the terminal functional group, the spacer being selected from: methylene (ethylene oxide), 1,1-difluoroethylene-(ethylene oxide), methylene-bis(ethylene oxide), 1,1-difluoroethylene-bis(ethylene oxide), methylene-tri(ethylene oxide), 1,1-difluoroethylene-tri(ethylene oxide), methylene-tetra(ethylene oxide), 1,1-difluoroethylene-tetra(ethylene oxide), methylene-penta(ethylene oxide), 1,1-difluoroethylene-penta(ethylene oxide), and a linear or branched hydrocarbon group, which is optionally fluorinated at the carbon atom connecting the spacer to the perfluoropolyether residue, comprising one or more carbamate groups or one or more amide groups, and optionally one or more cyclic moieties, the cyclic moieties including saturated cyclic moieties (such as cyclohexylene) and aromatic cyclic moieties (such as phenylene). Preferably, the perfluoropolyether surfactant is functionalized with one or more hydroxyl functional groups.

[0324] In a further preferred embodiment, the perfluoropolyether surfactant functionalized with one or more functional groups selected from the group consisting of hydroxyl, acrylate, methacrylate, and trialkoxysilyl is a compound of formula (VII) having an average molecular weight of about 1200 [g / mol] to about 2000 [g / mol]

[0325]

[0326] in

[0327] f and e are independently an integer selected from 1, 2 and 3;

[0328] FG 1 and FG 2 is independently selected from -OH, -OC(O)CH=CH2, and -OC(O)C(CH3)=CH2, and -Si(OR 20 )3 in the group consisting of terminal functional groups;

[0329] R 20 is a C1-C4 alkyl group;

[0330] -S1 - represents a single bond or a spacer selected from the following:

[0331]

[0332] in

[0333] -J 1 -Selected from

[0334]

[0335] in

[0336] j 1 is an integer between 1 and 12, preferably an integer between 4 and 10;

[0337] L 5 may be the same or different at each occurrence and is a straight chain or branched chain alkyl group containing 1 to 10 carbon atoms (such as methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, sec-butyl, tert-butyl, hexyl, octyl, and decyl), and preferably a straight chain or branched chain alkyl group containing 1 to 3 carbon atoms (such as methyl, ethyl, n-propyl, and isopropyl);

[0338] L 6 may be the same or different at each occurrence and is a straight chain or branched chain alkyl group containing 1 to 10 carbon atoms (such as methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, sec-butyl, tert-butyl, hexyl, octyl, and decyl), and preferably a straight chain or branched chain alkyl group containing 1 to 3 carbon atoms (such as methyl, ethyl, n-propyl, and isopropyl);

[0339] l 5 and l 6 are independently an integer between 4 and 10, preferably an integer between 0 and 1; and

[0340] -J 3 - is selected from -O-, -CH2-, -CH(CH3)-, and -C(CH3)2-;

[0341] -J 2 -Selected from

[0342]

[0343] a is an integer between 1 and 6, preferably an integer between 1 and 3; and

[0344] b is an integer between 1 and 6, preferably an integer between 2 and 4;

[0345] -S 2 - represents a single bond or a spacer selected from the following

[0346]

[0347] in

[0348] -J 4 -Selected from

[0349]

[0350] in

[0351] j 4 is an integer between 1 and 12, preferably an integer between 4 and 10;

[0352] L 7 may be the same or different at each occurrence and is a straight chain or branched chain alkyl group containing 1 to 10 carbon atoms (such as methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, sec-butyl, tert-butyl, hexyl, octyl, and decyl), and preferably a straight chain or branched chain alkyl group containing 1 to 3 carbon atoms (such as methyl, ethyl, n-propyl, and isopropyl);

[0353] L 8 may be the same or different at each occurrence and is a straight chain or branched chain alkyl group containing 1 to 10 carbon atoms (such as methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, sec-butyl, tert-butyl, hexyl, octyl, and decyl), and preferably a straight chain or branched chain alkyl group containing 1 to 3 carbon atoms (such as methyl, ethyl, n-propyl, and isopropyl);

[0354] l 7 and l 8 are independently an integer between 0 and 4, preferably an integer between 0 and 1; and

[0355] -J 6 - is selected from -O-, -CH2-, -CH(CH3)-, and -C(CH3)2-;

[0356] -J 5 -Selected from

[0357]

[0358] wherein r is an integer between 1 and 6, preferably an integer between 1 and 3; and

[0359] w is an integer between 1 and 6, preferably an integer between 2 and 4;

[0360] And wherein s and t are integers selected so that the average molecular weight of the compound of formula (VII) is about 1200 [g / mol] to about 2000 [g / mol].

[0361] Preferably, in the general formula (VII), FG 1 and FG 2 Independently of each other, they represent -OC(O)CH=CH2 or -OC(O)C(CH3)=CH2;

[0362] -S 1 -express wherein b has the meaning defined herein; and

[0363] -S 2 -express wherein w has the meaning defined herein.

[0364] Also preferably, in the general formula (VII), FG 1 and FG 2 It means -OH;

[0365] -S 1 - indicates a single bond or wherein a has the meaning defined herein;

[0366] -S 2 - indicates a single bond or wherein r has the meaning defined herein; and the sum of o and r is between 3 and 9.

[0367] Also preferably, in the general formula (VII), FG 1 and FG 2 Represents -Si(OR 20 )3;

[0368] R 20 is a C1-C4 alkyl group, preferably an ethyl group;

[0369] -S 1 -express wherein b has the meaning defined herein; and

[0370] -S 2 -express wherein w has the meaning defined herein. Therefore, the preferred perfluoropolyether surfactant is a compound of formula (VII-a)

[0371]

[0372] in

[0373] B and w are integers between 1 and 6, preferably between 2 and 4;

[0374] s is an integer between 2 and 6; and

[0375] q is an integer between 2 and 4.

[0376] A particularly suitable example of a perfluoropolyether surfactant functionalized with one or more functional groups selected from the group consisting of hydroxyl, acrylate, methacrylate and trialkoxysilyl is the poly(vinyl)ether surfactant commercially available from Solvay under the name E10H, MD700, AD1700, E-Series, and S10 is commercially available.

[0377] The UV-Vis radiation curable security ink claimed herein comprises e) about 3 wt-% to about 12 wt-% of a polyvinyl chloride copolymer, said polyvinyl chloride copolymer comprising at least 60 wt-% of vinyl chloride, preferably at least 63 wt-% of vinyl chloride. UV-Vis radiation curable security inks without polyvinyl chloride copolymers provide security features with unattractive colors, such as brown or dark brown, and low chromaticity values ​​C* when viewed under incident light, and are therefore not suitable for producing security features that appear metallic yellow under incident light.

[0378] Preferably, the polyvinyl chloride copolymer contains at most 90 wt-% vinyl chloride.

[0379] Preferably, the polyvinyl chloride copolymer containing at least 60 wt-% vinyl chloride is present in the security ink claimed herein in an amount of about 4.9 wt-% to about 11.6 wt-%, and most preferably about 6 wt-% to about 8.6 wt-%, wherein the weight percentages are based on the total weight of the UV-Vis radiation curable ink.

[0380] Preferably, the polyvinyl chloride copolymer is selected from the group consisting of: vinyl chloride-vinyl acetate copolymer, vinyl chloride-hydroxyalkyl acrylate copolymer such as vinyl chloride-2-hydroxypropyl acrylate copolymer, and vinyl chloride-hydroxyalkyl acrylate-Z-alkylene diacid, dialkyl ester copolymer such as vinyl chloride-2-hydroxypropyl acrylate-2-butenedioic acid (Z)-dibutyl ester copolymer. The polyvinyl chloride copolymer preferably has an average molecular weight of 3*10 4 g / mol~about 8*10 4 g / mol, the average molecular weight being determined by size exclusion chromatography using polystyrene as standard and tetrahydrofuran as solvent. Particularly suitable examples of the polyvinyl chloride copolymers of the present invention are those available from Wacker under the name H14 / 36, E22 / 48A, E 15 / 40A and H 40 / 50 is commercially available.

[0381] The UV-Vis radiation curable security ink claimed herein may contain f) up to about 25 wt-% of an organic solvent, the weight percentage being based on the total weight of the UV-Vis radiation curable ink. The boiling point of the organic solvent is above 100° C. Suitable organic solvents for the UV-Vis radiation curable ink described herein include, but are not limited to, ethyl 3-ethoxypropionate, 2-methoxy-1-methylethyl acetate, propylene glycol monomethyl ether, cyclopentanone, cyclohexanone, n-butanol, cyclohexanol, ethylene carbonate, propylene carbonate, butylene carbonate, and mixtures thereof.

[0382] In a preferred embodiment according to the invention, the UV-Vis radiation curable security ink is solvent-free. The use of solvent-free inks in industrial printing processes for valuable documents is very interesting because it prevents the emission of volatile organic components, which often have a negative impact on the environment and are harmful to human health.

[0383] The UV-Vis radiation curable security ink claimed herein may further include one or more photosensitizers and one or more photoinitiators described herein to achieve effective curing. Suitable examples of photosensitizers are known to those skilled in the art (e.g., in Table 8.1 of Industrial Photoinitiators, WA Green, CRC Press, 2010, page 170). Preferred photosensitizers are those that can achieve effective and rapid curing with a UV-LED light source, such as thioxanthone derivatives, anthracene derivatives, and naphthalene derivatives (e.g., 9,10-diethoxyanthracene sold as Anthracure UVS-1101 and 9,10-dibutyloxyanthracene sold as Anthracure UVS-1331, both sold by Kawasaki Kasei Chemicals Ltd) and cyclopentadienyl titanium derivatives (e.g., Irgacure 784 sold by BASF). Particularly preferred are thioxanthone derivatives, including but not limited to isopropyl-thioxanthone (ITX), 1-chloro-2-propoxy-thioxanthone (CPTX), 2-chloro-thioxanthone (CTX) and 2,4-diethyl-thioxanthone (DETX), and mixtures thereof. Optionally, thioxanthone photosensitizers can be used in oligomeric or polymeric form (such as OmnipolTX sold by IGM Resins, Genopol*TX-2 sold by Rahn, or Speedcure 7010 sold by Lambson). When present, one or more photosensitizers are preferably present in an amount of about 0.1 wt-% to about 2 wt-%, more preferably about 0.2 wt-% to about 1 wt-%, the weight percentages being based on the total weight of the UV-Vis radiation curable ink.

[0384] The UV-VIS radiation curable inks claimed herein may further include one or more defoaming agents in an amount of less than about 2 wt-%, preferably less than about 1 wt-%.

[0385] According to another aspect of the invention, a method for producing a security feature for protecting a valuable document, wherein the security feature appears blue when viewed in transmitted light and metallic yellow when viewed in incident light, comprises the following steps:

[0386] A) printing a UV-Vis radiation curable security ink as claimed herein onto a transparent or partially transparent area of ​​a substrate of a value document to provide an ink layer, preferably by screen printing, rotogravure printing, or flexographic printing; and

[0387] B) UV-Vis curing of the ink layer obtained in step B) to form a security feature.

[0388] The manufacturing method of the present invention claimed herein enables to obtain in a single printing step a security feature that presents a metallic yellow color under incident light and a blue color, particularly an intense to very intense blue color, under transmitted light. As used herein, the term "printing" refers to any printing method suitable for printing the UV-Vis radiation curable ink recorded herein on a substrate of a valuable document. In particular, the term "printing" refers to a printing method selected from the group consisting of: screen printing, rotogravure printing, flexographic printing, pad printing, inkjet printing and spray printing. Preferably, UV-Vis radiation curable security ink is printed on a transparent or partially transparent area of ​​a substrate of a valuable document by screen printing, rotogravure printing or flexographic printing, more preferably by screen printing.

[0389] As used herein, "a transparent or partially transparent area of ​​a substrate of a valuable document" refers to an area of ​​a substrate of a valuable document, wherein the area is characterized by an average transmittance in the visible light range of at least 50%, preferably at least 70%, and more preferably at least 90%. The transparent or partially transparent area of ​​the substrate and the remaining area of ​​the substrate can be made of the same material or different materials. Eliminating one or more layers in a multilayer structure, or applying a transparent or partially transparent material to a hole in a substrate made of a material different from the transparent or partially transparent material, provides a valuable document substrate, wherein the transparent or partially transparent area of ​​the substrate and the remaining area of ​​the substrate are made of different materials.

[0390] The material of valuable document substrate includes but is not limited to paper or other fiber materials such as cellulose, paper-containing materials, plastics and polymers, composite materials, and mixtures or combinations thereof. Typical paper, paper-like or other fiber materials are made of various fibers, and the fibers include but are not limited to Manila hemp, cotton, flax, wood pulp and blends thereof. As known to those skilled in the art, cotton and cotton / flax blends are preferably used for banknotes, while wood pulp is generally used for non-banknote security documents. Typical examples of plastics and polymers include polystyrene, polycarbonate, such as polyolefins such as polyethylene (PE) and polypropylene (PP) including biaxially oriented polypropylene (BOPP), polyamide (PA), such as poly (ethylene terephthalate) (PET), polyethylene terephthalate modified (PETG) including poly (ethylene glycol-co-1,4-cyclohexanedimethanol terephthalate), poly (1,4-butylene terephthalate) (PBT), and polyesters such as poly (ethylene 2,6-naphthoate) (PEN), and polyvinyl chloride (PVC). Typical examples of composite materials include, but are not limited to, a multilayer structure or laminate of paper and at least one plastic or polymer material such as those described above. Suitable materials for the transparent or partially transparent areas of the substrate include, but are not limited to, polystyrene, polycarbonate, such as polyolefins such as polyethylene (PE) and polypropylene (PP) including biaxially oriented polypropylene (BOPP), polyamides (PA), such as poly (ethylene terephthalate) (PET), polyethylene terephthalate modified (PETG) including poly (ethylene glycol-co-1,4-cyclohexanedimethanol terephthalate), poly (1,4-butylene terephthalate) (PBT), and polyesters such as poly (ethylene 2,6-naphthoate) (PEN), and polyvinyl chloride (PVC). The transparent or partially transparent area of ​​the substrate of the valuable document can carry a primer layer, on top of which UV-Vis radiation curable ink is printed. The undercoat layer can be obtained by UV-Vis curing a clear coat containing all the ingredients of the UV-Vis radiation curable ink described herein except for the silver nanoflakes.

[0391] In step B) of the manufacturing method of the invention claimed herein, the ink layer obtained in step A) is UV-Vis cured to form the security feature. As used herein, the term "UV-Vis curing" refers to the radiation curing of the ink layer by means of photopolymerization under the influence of irradiation with a wavelength component in the UV or in the UV and visible part of the electromagnetic spectrum (typically, 100 nm to 800 nm, preferably between 150 and 600 nm, and more preferably between 200 and 400 nm). Cationic curing monomers cure by a cationic mechanism consisting of UV-Vis light activation by one or more photoinitiators, which release cationic species, such as acids, which then initiate polymerization of the compounds to form a cured binder. Free radical curing monomers and oligomers cure by a free radical mechanism consisting of UV-Vis light activation by one or more photoinitiators, which release free radicals, which then initiate the polymerization process. Optionally, one or more photosensitizers may also be present. The photosensitizer is activated by one or more wavelengths emitted by a UV-Vis light source and reaches an excited state. The excited photosensitizer transfers energy to one or more photoinitiators (in free radical polymerization) or electrons (in cationic polymerization). Either process then initiates the polymerization process.

[0392] Preferably, step B) comprises exposing the ink layer obtained in step A) to UV-Vis light emitted by a UV-Vis light source, the UV-Vis light source being selected from the group consisting of: a mercury lamp, preferably a medium pressure mercury lamp, a UV-LED lamp, and a sequence thereof. A typical sequence comprises using one or more UV-LED lamps in a first step to partially cure the UV-Vis radiation composition, and using one or more medium pressure mercury lamps in a second step. Mercury lamps advantageously emit over a wide range of wavelengths within the UV-A, UV-B and UV-C ranges. Therefore, there is a large selection of photoinitiators or combinations of photoinitiators / photosensitizers whose absorption spectra match at least one emission band of the mercury lamp. UV-LEDs have a more limited wavelength range, so that only a limited selection of photoinitiators or combinations of photoinitiators / photosensitizers are sufficiently effective at industrial printing speeds. On the other hand, UV-LEDs are less expensive, require less energy (in particular, they require much less demanding heat dissipation systems), are less prone to ozone formation, and have a much longer lifetime.

[0393] In order to provide soil resistance to the value document and / or protect the security feature from physical and chemical attacks from the environment, the manufacturing method claimed herein preferably further comprises steps C) and D) performed after step B):

[0394] C) applying, preferably by a printing method, a curable protective varnish to the substrate to form a varnish layer;

[0395] D) curing the varnish layer obtained in step C) to form a protective coating.

[0396] Examples of suitable curable protective varnishes used in step C) and / or methods of applying the curable protective varnishes to a substrate and curing the varnish layer are described in International Patent Application Publication No. WO2020234211A1, International Patent Application Publication No. WO2013127715A2 and International Patent Application Publication No. WO2014067715A1.

[0397] Preferably, the valuable document is selected from banknotes, contracts, bills, checks, vouchers, tax stamps, agreements, identity documents such as passports, identity cards, visas, driver's licenses, bank cards, credit cards, transaction cards, pass documents, and cards, admission tickets, public transportation tickets, diplomas, and academic titles. More preferably, the valuable document is a banknote. The security ink claimed for protection herein can also be used to produce security features directly on valuable commercial goods. The term "valuable commercial goods" refers to packaging materials, particularly packaging materials for medicines, cosmetics, electronic products or food industries, which can be protected from counterfeiting and / or illegal duplication to guarantee the contents of the package, such as genuine drugs.

[0398] Example

[0399] The invention will now be described in more detail with reference to non-limiting examples.The following Examples E1 - E26 and Comparative Examples C1 - C8 provide further details of the preparation of the UV-Vis radiation curable screen printable security inks described herein and the optical properties of the security features obtained therefrom.

[0400] A. Analytical Methods

[0401] A-1. UV-Vis spectroscopy

[0402] UV-Vis spectra of the dispersions were recorded on a Varian Cary 50 UV-Vis spectrophotometer, the concentration of the dispersion was such that an optical density of 0.3 to 1.5 was obtained on a 1 cm pathlength.

[0403] A-2.TEM analysis

[0404] TEM analysis of the dispersions was performed on an EM 910 instrument from ZEISS in bright field mode at an electron beam acceleration voltage of 100 kV. At least 2 representative images with different magnification scales were recorded to characterize the main particle morphology of each sample.

[0405] The average diameter of the silver nanosheets was determined by transmission electron microscopy (TEM) based on the measurement of at least 300 randomly selected silver nanosheets oriented parallel to the plane of the transmission electron microscopy image (TEM) using Fiji image analysis software, wherein the diameter of the silver nanosheet is the largest dimension of the silver nanosheet oriented parallel to the plane of the transmission electron microscopy image (TEM).

[0406] The average thickness of the silver nanosheets was determined by transmission electron microscopy (TEM) based on manual measurements of at least 50 randomly selected silver nanosheets oriented perpendicular to the plane of the TEM image, wherein the thickness of the silver nanosheets is the maximum thickness of the silver nanosheets.

[0407] B. Preparation and Characterization of Ag Nanosheet Dispersions D1 and D2

[0408] B-1. Synthesis of raw materials

[0409] In a 1 L double-walled glass reactor equipped with an anchor stirrer, 365 g of deionized water were cooled to +2° C. 13.62 g of sodium borohydride were added and the mixture was cooled to −1° C. under stirring at 250 revolutions per minute (RPM, solution A).

[0410] In a 0.5 L double-walled glass reactor equipped with an anchor stirrer, 132 g of deionized water and 4.8 g of MPEG-5000-thiol were mixed and the mixture was stirred at room temperature for 10 minutes. 72 g of the product of Example A3 of WO2006074969 was added and the resulting mixture was stirred for another 10 minutes at room temperature to homogenize. A solution of 30.6 g of silver nitrate in 30 g of deionized water was added in one go and the mixture was stirred for 10 minutes to give an orange-brown viscous solution. To this solution was added 96 g of deionized water followed by 3 g of Struktol SB 2080 defoamer pre-dispersed in 36 g of deionized water. The resulting mixture was cooled to 0° C. with stirring at 250 RPM (Solution B).

[0411] Afterwards, solution B was added to solution A below the liquid surface via a cooled (0° C.) feeding tube using a peristaltic pump at a constant rate over 2 hours to obtain a dispersion of spherical silver nanosheets. During pumping, solution A was stirred at 250 RPM.

[0412] After the feeds were complete, the reaction mixture was warmed to +5°C within 15 minutes and a solution of 862 mg of KCl in 10 g of deionized water was added in one portion, followed by 9.6 g of ethylenediaminetetraacetic acid (EDTA) in 4 equal portions at 10 minute intervals.

[0413] After the last portion of EDTA was added, the reaction mixture was stirred at +5°C for 15 minutes, then warmed to 35°C over 30 minutes and stirred at this temperature for 1 hour. At this point, hydrogen evolution was complete.

[0414] 3.0 mL of a 30% w / w aqueous ammonia solution was added, followed by 5.76 g of solid NaOH, and the mixture was stirred at 35° C. for 15 minutes. 180 mL of a 50% w / w aqueous hydrogen peroxide solution was then added to the reaction mixture subsurface at a constant rate over 4 hours using a peristaltic pump while stirring at 250 RPM while maintaining the temperature at 35° C. This resulted in a dark blue dispersion of silver nanosheets, which was cooled to room temperature. 1.23 g of the compound of formula (mixture of CAS 80584-88-9 and 80584-89-0), and the mixture was stirred at room temperature for 1 hour.

[0415] B-2. Separation and purification of Ag nanosheets

[0416] B-2a. First decantation

[0417] 9.6 g of sodium dodecyl sulfate was added to the reaction mixture, and then about 25 g of anhydrous sodium sulfate powder was added in batches under stirring until the transmission color of the dispersion changed from blue to pink. The mixture was then kept at room temperature without stirring for 24 hours to allow the condensed nanosheets to precipitate at the bottom of the reactor.

[0418] 890 g of the supernatant was pumped out of the reactor using a peristaltic pump, and 890 g of deionized water was added to the reactor. The mixture in the reactor was stirred at room temperature for 1 hour to redisperse the coagulated particles.

[0419] B-2b. Second decantation

[0420] About 64 g of anhydrous sodium sulfate powder was added in batches under stirring until the transmission color of the dispersion changed from blue to pale yellow pink. The mixture was then kept at room temperature without stirring for 12 hours to allow the condensed nanosheets to settle at the bottom of the reactor. 990 g of the supernatant was pumped out of the reactor with a peristaltic pump, and 90 g of deionized water was added to the reactor. The resulting mixture was stirred at room temperature for 30 minutes to redisperse the condensed particles.

[0421] B-2c. Ultrafiltration in water

[0422] The resulting dispersion of Ag nanosheets was ultrafiltered using a Millipore Amicon 8400 stirred ultrafiltration cell. The dispersion was diluted to 400 g weight with deionized water and ultrafiltered to a final volume of about 50 mL using a polyethersulfone (PES) membrane with a 300 kDa cutoff. The process was repeated 4 times in total to provide 60 g of a dispersion of Ag nanosheets in water. After the ultrafiltration was complete, 0.17 g of the compound of the formula

[0423]

[0424] (mixture of CAS 80584-88-9 and 80584-89-0) was added to the dispersion.

[0425] Ag content 28.9% w / w; yield based on total silver content about 89%; solid content (at 250°C) 33.5% w / w; silver purity based on solid content at 250°C is 86% w / w.

[0426] B-2d. Ultrafiltration in isopropanol

[0427] The dispersion was further ultrafiltered in isopropanol. The 60g Ag nanosheet dispersion obtained after ultrafiltration in water was placed in a Millipore Amicon 8400 stirred ultrafiltration cell and diluted to 300g weight with isopropanol. Using a polyethersulfone (PES) membrane with a 500kDa cutoff, the dispersion was ultrafiltered to a volume of about 50mL. The process was repeated 4 times in total to provide a 72g Ag nanosheet dispersion in isopropanol.

[0428] Ag content: 24.1% w / w; solid content (at 250°C): 25.7% w / w; silver purity based on the solid content at 250°C: 93.5% w / w.

[0429] When the Ag concentration is 9.8*10 -5 UV-Vis-NIR spectra were recorded in water of M. max =700nm; maximum extinction coefficient ε =10200L / (cm*mol Ag), FWHM =340nm.

[0430] The average diameter of the silver nanosheets was 93±40 nm, and the average thickness of the silver nanosheets was 16±2.5 nm.

[0431] B-3. ​​Preparation of Dispersion D1

[0432] a) Surface modification of Ag nanosheets

[0433] At 23°C, under an argon atmosphere, 50 g (12.85 g solid) of the Ag nanosheet dispersion obtained as described in item B-2d was placed in a 250 mL round bottom flask. 2.05 g of a 5% w / w solution of carbon disulfide in anhydrous ethanol was added and the mixture was stirred for 5 minutes, followed by the addition of 2.77 g of a 5% w / w solution of diethanolamine in anhydrous ethanol. The mixture was stirred at 23°C for 1 hour, followed by the addition of 2.77 g of a 5% w / w solution of diethanolamine in anhydrous ethanol, and stirring was continued for 30 minutes.

[0434] When the Ag concentration is 9.8*10 -5 UV-Vis-NIR spectra were recorded in water of M. max =704nm.

[0435] b) Solvent switching

[0436] 15.0 g of ethyl 3-ethoxypropionate were added to the dispersion obtained in step a). The resulting mixture was concentrated on a rotary evaporator at a pressure of 40 mbar and a bath temperature of 40° C. until no more solvent was distilled off. The weight of the resulting dispersion was adjusted to 32.1 g by adding ethyl 3-ethoxypropionate (corresponding to a calculated total solids content of 41.2% w / w).

[0437] B-4 Preparation of Dispersion D2

[0438] a) Surface modification of Ag nanosheets

[0439] At 23°C, under an argon atmosphere, 50 g (12.85 g solid) of the Ag nanosheet dispersion obtained as described in item B-2d was placed in a 250 mL round bottom flask. 2.05 g of a 5% w / w solution of carbon disulfide in anhydrous ethanol was added and the mixture was stirred for 5 minutes, followed by the addition of 2.77 g of a 5% w / w solution of diethanolamine in anhydrous ethanol. The mixture was stirred at 23°C for 1 hour, followed by the addition of 2.77 g of a 5% w / w solution of diethanolamine in anhydrous ethanol, and stirring was continued for 30 minutes.

[0440] When the Ag concentration is 9.8*10 -5 UV-Vis-NIR spectra were recorded in water of M. max =704nm.

[0441] b) Solvent switching

[0442] 15.0 g of 7-oxabicyclo[4.1.0]hept-3-ylmethyl 7-oxabicyclo[4.1.0]heptane-3-carboxylate (CAS: 2386-87-0) are added to the dispersion obtained in step a). The resulting mixture is concentrated on a rotary evaporator at a pressure of 40 mbar and a bath temperature of 40° C. until no more solvent is distilled off. The weight of the resulting dispersion is adjusted to 32.1 g by adding 7-oxabicyclo[4.1.0]hept-3-ylmethyl 7-oxabicyclo[4.1.0]heptane-3-carboxylate (CAS: 2386-87-0) (corresponding to a calculated total solids content of 41.2% w / w).

[0443] C. Preparation of Examples (E1-E26), Comparative Examples (C1-C8) and Printed Security Features Thereof

[0444] Description of ingredients of Examples (E1-E26) and Comparative Examples (C1-C8)

[0445] Table 1. Ingredients

[0446]

[0447]

[0448]

[0449] a) 41.2 wt-% Ag nanosheets stabilized with diethanolammonium dihydroxyethyl dithiocarbamate in ethyl 3-ethoxypropionate (763-69-9)

[0450] b) 41.2 wt-% Ag nanosheets stabilized with diethanolammonium dihydroxyethyl dithiocarbamate in 7-oxabicyclo[4.1.0]hept-3-ylmethyl 7-oxabicyclo[4.1.0]heptane-3-carboxylate (Uvacure 1500, 2386-87-0)

[0451] C1. Preparation of security inks (E1-E8) according to the invention and dichroic security features thereof

[0452] C1a. Preparation of mixed safety inks E1–E8

[0453] The ingredients provided in Table 2a below were individually mixed and dispersed using a Dispermat CV-3 at 2000 rpm for 10 minutes at room temperature to obtain 50 g of inks E1-E8.

[0454] Table 1a. Composition of UV-Vis radiation curable screen printing inks E1-E8

[0455]

[0456]

[0457] a) 41.2 wt-% Ag nanosheets stabilized with diethanolammonium dihydroxyethyl dithiocarbamate in ethyl 3-ethoxypropionate (763-69-9)

[0458] b) 41.2 wt-% Ag nanosheets stabilized with diethanolammonium dihydroxyethyl dithiocarbamate in 7-oxabicyclo[4.1.0]hept-3-ylmethyl 7-oxabicyclo[4.1.0]heptane-3-carboxylate (Uvacure 1500, 2386-87-0)

[0459] C1b. Preparation of security features

[0460] UV-Vis radiation curable screen printable hybrid security inks E1-E8 were applied individually to a transparent polymer substrate (PET) using a 160 lines / cm screen (405 mesh). RN, thickness 50 μm, supplied by Pütz GmbH + Co. Folien KG). The size of the printed pattern was 5 cm×5 cm. 10 seconds after the printing step, the printed substrate sheet was passed through a UV-Vis light (two lamps: iron-doped mercury lamp 200 W / cm 2 + Mercury lamp 200W / cm 2 ) at a speed of 100 m / min to cure independently at room temperature to produce the security features.

[0461] C1c. Results of security features (optical properties)

[0462] The optical properties of each security feature obtained in item C1b were evaluated independently in reflection, in transmission and visually using the three tests described below. The results are summarized in Table 1c.

[0463] Reflection measurements were performed using a goniometer (Goniospektrometer Codec WI-10 5&5 from Phyma GmbH Austria). The L*a*b* values ​​of the printed security feature were determined on the side of the printed transparent polymer substrate at an illumination angle of 22.5° at 0° to the normal. The C* value (chromaticity, a measure corresponding to color intensity or color saturation) was calculated from the a* and b* values ​​according to the CIELAB (1976) color space, where:

[0464]

[0465] The C* values ​​(reflection 22.5 / 0°) are shown in Table 1c below.

[0466] Transmission measurements were performed using a Datacolor 650 spectrophotometer (parameters: integrating sphere, diffuse illumination (pulsed xenon D65) and 8° observation, analyzer SP2000 with dual 256 diode array for 360-700 nm wavelength range, transmission sampling aperture size 22 mm). The C* values ​​(transmission 8°) are shown in Table 1c below.

[0467] Visual assessments were made by observing each security feature with the naked eye under reflection from a diffuse light source (e.g., light shining from a window without direct sunlight, with the observer facing the wall opposite the window). The following colors were observed:

[0468] - dark brown to brown with a matte appearance and no metallic effect;

[0469] - Gold (ie metallic yellow) with a lustrous appearance and a metallic effect. The metallic effect occurs at chromaticity values ​​C* above about 20 in reflection 22.5 / 0°.

[0470] A visual assessment was also performed, observing each security feature in transmission with the naked eye. The following colors were observed:

[0471] - Dark blue: The blue color is faint (but visible);

[0472] Blue (chromaticity value C* at transmission 8° higher than or equal to about 20) to dark blue (chromaticity value C* at transmission 8° higher than or equal to 30): intense to very intense blue shade.

[0473] As shown in Table 1c, the security features obtained with the inks according to the invention (Examples E1-E8) appear golden in reflection and blue to dark blue in transmission.

[0474] Table 1c. Color properties of security features obtained with inks E1-E8

[0475] E1 E2 E3 E4 E5 E6 E7 E8 C*(reflection 22.5 / 0°) 31 35 40 34 24 25 28 24 C*(transmission 8°) 36 36 40 42 43 39 48 41 Color (Reflection) gold gold gold gold gold gold gold gold Color (Transmission) Dark Blue Dark Blue Dark Blue Dark Blue Dark Blue Dark Blue Dark Blue Dark Blue

[0476] As shown in Table 1c, the solvent-containing hybrid security inks E1-E7 according to the present invention and the solvent-free hybrid security ink E8 according to the present invention comprising a mixture of alicyclic epoxide and a free radical curable monomer / oligomer, or a mixture of alicyclic epoxide, a free radical curable monomer / oligomer and a cation curable monomer provide security features with excellent visual effects and high chromaticity values ​​C* in both reflected light and transmitted light.

[0477] C2. Preparation of security inks (E9-E15) according to the invention and dichroic security features thereof

[0478] C2a. Preparation of cationic curable safety inks E9–E15

[0479] The ingredients provided in Table 2a below were mixed and dispersed using a Dispermat CV-3 at 2000 rpm for 10 minutes at room temperature to obtain 50 g of each of inks E9 - E15.

[0480] Table 2a. Composition of UV-Vis radiation curable screen printing inks E9 - E15.

[0481]

[0482] a) 41.2 wt-% Ag nanosheets stabilized with diethanolammonium dihydroxyethyl dithiocarbamate in ethyl 3-ethoxypropionate (763-69-9)

[0483] b) 41.2 wt-% Ag nanosheets stabilized with diethanolammonium dihydroxyethyl dithiocarbamate in 7-oxabicyclo[4.1.0]hept-3-ylmethyl 7-oxabicyclo[4.1.0]heptane-3-carboxylate (Uvacure 1500, 2386-87-0)

[0484] C2b. Preparation of security features

[0485] UV-Vis radiation curable screen printing inks E9–E15 were applied individually to a transparent polymer substrate (PET) using a 160 lines / cm screen (405 mesh). RN, thickness 50 μm, supplied by Pütz GmbH + Co. Folien KG). The size of the printed pattern was 5 cm×5 cm. 10 seconds after the printing step, the printed substrate sheet was passed through a UV-Vis light (two lamps: iron-doped mercury lamp 200 W / cm 2 + Mercury lamp 200W / cm 2 ) at a speed of 100 m / min to cure independently at room temperature to produce the security features.

[0486] C2c. Security feature results (optical properties)

[0487] The optical properties of the security feature obtained in item C2b are evaluated independently in reflection, in transmission and visually using the test described in item C1c.

[0488] The colors in reflection and transmission as well as the C* values ​​(reflection 22.5 / 0° and transmission 8°) exhibited by security features prepared using comparative inks E9 - E15 according to the invention are shown in Table 2c (below).

[0489] Table 2c. Color properties of security features obtained with inks E9-E15

[0490]

[0491] As demonstrated in Table 2c, the cationically curable solvent-free safety inks E9-E12 according to the present invention and the cationically curable solvent-containing safety inks E13-E15 according to the present invention comprising alicyclic epoxides, or alicyclic epoxides and other cationically curable monomers provide security features with excellent visual effects and high chromaticity values ​​C* in both reflected and transmitted light.

[0492] C3. Study of the influence of surfactants on the optical properties presented by security features (comparative inks C1-C7 and inks E16-E18 according to the invention)

[0493] In order to evaluate the influence of surfactants on the optical properties exhibited by the security feature, comparative inks C1 - C7 and inks E16 - E18 according to the invention were prepared.

[0494] C3a. Preparation of inks C1–C7 and E16–E18

[0495] The ingredients provided in Table 3a below were mixed and dispersed using a Dispermat CV-3 at 2000 rpm for 10 minutes at room temperature to obtain 50 g of each of inks C1 - C7 and E16 - E18.

[0496] Table 3a. Composition of UV-Vis radiation curable screen printing inks C1 - C7 and E18 - E20.

[0497]

[0498] a) 41.2 wt-% Ag nanosheets stabilized with diethanolammonium dihydroxyethyl dithiocarbamate in ethyl 3-ethoxypropionate (763-69-9)

[0499] C3b. Preparation of security features

[0500] UV-Vis radiation curable screen printing inks C1-C7 and E16-E18 were independently applied to a transparent polymer substrate (PET) using a 160 lines / cm screen (405 mesh). RN, thickness 50 μm, supplied by Pütz GmbH + Co. Folien KG). The size of the printed pattern was 5 cm×5 cm. 10 seconds after the printing step, the printed substrate sheet was passed through a UV-Vis light (two lamps: iron-doped mercury lamp 200 W / cm2 + Mercury lamp 200W / cm 2 ) at a speed of 100 m / min to cure independently at room temperature to produce the security features.

[0501] C3c. Results of security features (optical properties)

[0502] The optical properties of the security feature obtained in item C3b are evaluated independently in reflection, in transmission and visually using the test described in item C1c.

[0503] The colors exhibited in reflection and transmission as well as the C* values ​​(reflection 22.5 / 0° and transmission 8°) for security features prepared using inks C1 - C7 and E16 - E18 are shown in Table 3c below.

[0504] Table 3c. Color characteristics of security features obtained with inks C1-C7 and E16-E18

[0505]

[0506] As shown in Table 3c, the security features obtained with inks according to the invention comprising inks of perfluoropolyether surfactants functionalized with hydroxyl groups (Fluorolink E10H: ink E16), (meth)acrylate groups (Fluorolink MD700: ink E17), or silane groups (Fluorolink S10: ink E18) appear golden in reflection and dark blue in transmission. In contrast, security features obtained from inks comprising a perfluoropolyether surfactant lacking said functional group (Fluorolink F10: comparative ink C1), or surfactants lacking a perfluoropolyether chain such as BYK 330 (Comparative ink C2), BYK 371 (Comparative ink C3), TEGORAD 2300 (Comparative ink C4), TEGO RAD 2700 (Comparative ink C5), Dynasylan F8815 (Comparative ink C6) and Dynasylan F8261 (Comparative ink C7) appear dark blue to blue in transmission, but appear dark brown to brown with low chromaticity values ​​in reflection. The dark brown to brown color with low chromaticity values ​​in reflection is not noticeable and, therefore, is not suitable for dichroic security features for protecting valuable documents.

[0507] C4. Study of the influence of the amount of perfluoropolyether surfactant on the optical properties presented by the security feature (comparative ink C8 and inks E19-E23 according to the invention)

[0508] In order to evaluate the effect of the amount of perfluoropolyether surfactant as described herein on the optical properties exhibited by the security feature, ink C8 and inks E19 - E23 according to the invention were prepared as follows.

[0509] C4a. Preparation of inks C8 and E19–E23

[0510] The ingredients provided in Table 4a below were mixed and dispersed using a Dispermat CV-3 at 2000 rpm for 10 minutes at room temperature to obtain 50 g of each of inks C8 and E19 - E23.

[0511] Table 4a. Composition of UV-Vis radiation curable screen printing inks C8 and E19-E23.

[0512]

[0513] a) 41.2 wt-% Ag nanosheets stabilized with diethanolammonium dihydroxyethyl dithiocarbamate in ethyl 3-ethoxypropionate (763-69-9)

[0514] C4b. Preparation of security features

[0515] UV-Vis radiation curable screen printing inks C8 and E19–E23 were independently applied to a transparent polymer substrate (PET) using a 160 lines / cm screen (405 mesh). RN, thickness 50 μm, supplied by Pütz GmbH + Co. Folien KG). The size of the printed pattern was 5 cm×5 cm. 10 seconds after the printing step, the printed substrate sheet was passed through a UV-Vis light (two lamps: iron-doped mercury lamp 200 W / cm 2 + Mercury lamp 200W / cm 2 ) at a speed of 100 m / min to cure independently at room temperature to produce the security features.

[0516] C4c. Security feature results (optical properties)

[0517] The optical properties of the security feature obtained in item C4b are evaluated independently in reflection, in transmission and visually using the test described in item C1c.

[0518] The colors exhibited in reflection and transmission as well as the C* values ​​(reflection 22.5 / 0° and transmission 8°) for security features prepared using inks C8 and E19 - E23 are shown in Table 4c below.

[0519] Table 4c. Color properties of security features obtained with inks C8 and E19–E23

[0520] C8 E19 E20 E21 E22 E23 The amount of surfactant 0 0.05 0.5 1 2.5 5 C*(reflection 22.5 / 0°) 2 32 33 33 35 31 C*(transmission 8°) 24 47 43 40 36 42 Color (Reflection) Dark Brown gold gold gold gold gold Color (Transmission) blue Dark Blue Dark Blue Dark Blue Dark Blue Dark Blue

[0521] As shown in Table 4c, the use of a perfluoropolyether surfactant as described herein (such as Fluorolink E10H used in inks E19-E23) in an amount of about 0.05 wt-% to about 5 wt-% ensures that a security feature is obtained that exhibits a golden yellow color with high chromaticity values ​​in reflection and a dark blue color in transmission (inks E19-E23). In contrast, the security feature obtained in the experiment with ink C8 without surfactant exhibits a dark brown to brown color with low chromaticity values ​​in reflection. This color is not striking to the layman and cannot be used as a security feature for protecting valuable documents.

[0522] C5. Study of the influence of the type of polyvinyl chloride copolymer on the optical properties presented by the security feature (inks E1 and E24-E26 according to the invention)

[0523] In order to evaluate the influence of the type of polyvinyl chloride copolymer on the optical properties exhibited by the security feature, inks E1 and E24 - E26 according to the invention were prepared as follows.

[0524] C5a. Preparation of inks E1 and E24–E26

[0525] The ingredients provided in Table 5a below were mixed and dispersed using a Dispermat CV-3 at 2000 rpm for 10 minutes at room temperature to obtain 50 g of each of inks E1 and E24 - E26.

[0526] Table 5a. Composition of UV-Vis radiation curable screen printing inks E1 and E24 - E26.

[0527]

[0528] a) Polyvinyl chloride / polyvinyl acetate (85.6% / 14.4%) (9003-22-9), K value 35±1, molecular weight 3-4·10 4 Dalton (Wacker, size exclusion chromatography)

[0529] b) Polyvinyl chloride / polyvinyl acetate (63% / 37%) (9003-22-9), K value 50±1, molecular weight 6-8·10 4 Dalton

[0530] c) Polyvinyl chloride / (acrylic acid / 1,2-propylene glycol copolymer) (57495-45-1) (84% / 16%), K value 39±1, molecular weight 4-5·10 4 Dalton

[0531] d)Polyvinyl chloride / (acrylic acid / 1,2-propylene glycol / dibutyl butyl ester copolymer) (114653-42-8) (75% / 25%), K value 48±1, molecular weight 6-8·10 4 Dalton

[0532] e) 41.2 wt-% Ag nanosheets stabilized with diethanolammonium dihydroxyethyl dithiocarbamate in ethyl 3-ethoxypropionate (763-69-9)

[0533] C5b. Preparation of security features

[0534] UV-Vis radiation curable screen printing inks E1 and E24–E26 were independently applied to a transparent polymer substrate (PET) using a 160 lines / cm screen (405 mesh). RN, thickness 50 μm, supplied by Pütz GmbH + Co. Folien KG). The size of the printed pattern was 5 cm×5 cm. 10 seconds after the printing step, the printed substrate sheet was passed through a UV-Vis light (two lamps: iron-doped mercury lamp 200 W / cm 2 + Mercury lamp 200W / cm 2 ) at a speed of 100 m / min to cure independently at room temperature to produce the security features.

[0535] C5c. Results of security features (optical properties)

[0536] The optical properties of the security feature obtained in item C5b are evaluated independently in reflection, in transmission and visually using the test described in item C1c.

[0537] The colors exhibited in reflection and transmission as well as the C* values ​​(reflection 22.5 / 0° and transmission 8°) for security features prepared using inks El and E24 - E26 are shown in Table 5c below.

[0538] Table 5c. Color properties of security features obtained with inks E1 and E24-E26

[0539]

[0540] As demonstrated by the optical properties of the security feature shown in Table 5c, the security inks claimed herein comprising a polyvinyl chloride copolymer containing at least about 60 wt-%, preferably at least about 63 wt-%, of vinyl chloride provide a security feature that appears blue to dark blue in reflection and metallic yellow in reflection.

[0541] C6. Study on the stability of the UV-Vis radiation curable safety ink E2 according to the present invention by accelerated aging experiment

[0542] In order to evaluate the stability of the ink according to the invention over time, 10 g of ink E2 (described in Table 1a) were placed in a cup (SpeedMixer available from Hauschild & Co. KG). TM The samples of ink E2 stored in the oven were cooled at room temperature for 6 hours each month and then applied to a transparent polymer substrate (PET) using a 160 line / cm screen (405 mesh). RN, thickness 50 μm, supplied by Pütz GmbH + Co. Folien KG). The size of the printed pattern was 5 cm×5 cm. 10 seconds after the printing step, the printed substrate sheet was passed through a UV-Vis light (two lamps: iron-doped mercury lamp 200 W / cm 2 + Mercury lamp 200W / cm 2 ) at a speed of 100 m / min for curing at room temperature to produce the security features. The optical properties of the security features obtained each month were evaluated independently in reflection and visually using the test described in item C1c. Table 6 summarizes the colors presented by the security features in reflection and transmission as well as the C* values ​​(reflection 22.5 / 0°).

[0543] Table 6. Color characteristics of security features

[0544]

[0545] a) The security feature was produced with ink E2 which was freshly prepared according to the invention.

[0546] As demonstrated by the security feature optical properties shown in Table 6, ink E2 according to the invention remains stable at elevated temperatures for extended periods of time, indicating outstanding storage stability at room temperature.

Claims

1. A UV-Vis radiation curable security ink for producing a security feature which appears blue when viewed in transmitted light and metallic yellow when viewed in incident light, wherein the ink comprises: a) 7.5 wt% to 20 wt% of silver nanoflakes having an average diameter in the range of 50 to 150 nm with a standard deviation of less than 60%, an average thickness in the range of 5 to 30 nm with a standard deviation of less than 50%, and an average aspect ratio greater than 2.0, wherein the average diameter is determined by transmission electron microscopy, and the average thickness is determined by transmission electron microscopy, and The silver nanosheets have a surface stabilizer of general formula (I) in Residue R A is a C2-C4 alkyl group substituted with a hydroxyl group; Residue R B is selected from C1-C4 alkyl, and C2-C4 alkyl substituted with hydroxyl; and Cat + For the general formula + NH2R C R D The ammonium cation, The residue R C is a C2-C4 alkyl group substituted with a hydroxy group; and Residue R D is selected from C1-C4 alkyl, and C2-C4 alkyl substituted with hydroxyl; b) 45 wt% to 80 wt% of a cycloaliphatic epoxide, or a mixture of a cycloaliphatic epoxide and one or more UV-Vis radiation curable compounds; c) one or more cationic photoinitiators; d) a perfluoropolyether surfactant functionalized with one or more functional groups selected from the group consisting of hydroxyl, acrylate, methacrylate, and trialkoxysilyl; e) 3 wt% to 12 wt% of a polyvinyl chloride copolymer, the polyvinyl chloride copolymer comprising at least 60 wt% of vinyl chloride; and optionally f) up to 25 wt% of an organic solvent; The weight percentages are based on the total weight of the UV-Vis radiation curable security ink.

2. The UV-Vis radiation curable security ink according to claim 1, wherein the security ink is selected from the group consisting of screen printing security ink, rotogravure printing security ink, and flexographic printing security ink.

3. The UV-Vis radiation curable security ink according to claim 1 or 2, wherein the average diameter of the silver nanosheets is in the range of 70 to 120 nm with a standard deviation of less than 50%, the average thickness of the silver nanosheets is in the range of 8 to 25 nm with a standard deviation of less than 30%, and the average aspect ratio of the silver nanosheets is higher than 2.

5.

4. The UV-Vis radiation curable security ink according to claim 1 or 2, wherein the surface stabilizer of the general formula (I) is present in an amount of 0.5% to 5% by weight of the silver nanoplatelets of a).

5. The UV-Vis radiation curable security ink according to claim 1 or 2, wherein the residue R A and R B are independently C2-C4 alkyl substituted with hydroxy.

6. The UV-Vis radiation curable security ink according to claim 1 or 2, wherein the silver nanoplatelets carry a further surface stabilizer of the general formula (II) in Indicates bonding with silver; R 1 H, C1-C18 Alkyl, phenyl, C1-C8 alkylphenyl, or CH2COOH; R 2 , R 3 , R 4 , R 5 , R 6 and R 7 are independently H, C1-C8 alkyl, or phenyl; Y is O or NR 8 ; R 8 is H, or C1-C8 alkyl; k1 is an integer in the range of 1 to 500; k2 and k3 are independently 0 or an integer in the range of 1 to 250; k4 is 0 or 1; and k5 is an integer in the range of 1 to 5.

7. The UV-Vis radiation curable security ink according to claim 1 or 2, wherein the silver nanoplatelets carry a further surface stabilizer of formula (III) in R 17a , R 17b and R 17c are independently H or methyl; R 18a and R 18b is H, or methyl; R 19a is a saturated or unsaturated, linear or branched alkyl group having 1 to 22 carbon atoms; R 19b For R c -[O-CH2-CH2-] c -O-; R 19c for -C(=O)-NH-(CH2) y NR 15 R 16 ,or -C(=O)-NH-(CH2) y N + HR 15 R 16 An - ; in An - It is the anion of a monovalent organic or inorganic acid; y is an integer from 2 to 10; R 15 is a saturated or unsaturated, linear or branched alkyl group having 1 to 22 carbon atoms, R 16 is a saturated or unsaturated, linear or branched alkyl group having 1 to 22 carbon atoms, R c is a saturated or unsaturated, linear or branched alkyl group having 1-22 carbon atoms, or an alkylaryl or dialkylaryl group having up to 24 carbon atoms, and c is 1 to 150, and y1, y2 and y3 are each independently an integer of 1 to 200.

8. The UV-Vis radiation curable security ink according to claim 1 or 2, wherein the silver nanoplatelets carry a further surface stabilizer of formula (IV) in R 9 A hydrogen atom or a -CHR 11 -N(R 12 )(R 13 ) R 10 is a hydrogen atom, a halogen atom, a C1-C8 alkoxy group, or a C1-C8 alkyl group; R 11 is H, or C1-C8 alkyl; and R 12 and R 13 are independently C1-C8 alkyl, C1-C8 alkyl substituted with hydroxyl, or a group of the formula -[(CH2CH2)-O] n1 -CH2CH2-OH group, wherein n1 is 1 to 5.

9. The UV-Vis radiation curable security ink according to claim 1 or 2, wherein the one or more UV-Vis radiation curable compounds include one or more cationic curable monomers selected from the group consisting of vinyl ethers, propenyl ethers, cyclic ethers other than alicyclic epoxides, lactones, cyclic thioethers, vinyl thioethers, propenyl thioethers, hydroxyl-containing compounds, and mixtures thereof.

10. The UV-Vis radiation curable security ink according to claim 1 or 2, wherein the one or more UV-Vis radiation curable compounds include one or more free radical curable monomers and / or oligomers, and the UV-Vis radiation curable ink further comprises g) one or more free radical photoinitiators.

11. The UV-Vis radiation curable security ink according to claim 1 or 2, wherein the UV-Vis radiation curable security ink comprises a perfluoropolyether surfactant in an amount of 0.025 wt% to 5 wt%, wherein the weight percentage is based on the total weight of the UV-Vis radiation curable security ink.

12. The UV-Vis radiation curable security ink according to claim 1 or 2, wherein the UV-Vis radiation curable security ink is solvent-free.

13. A method for producing a security feature for protecting a valuable document, wherein the security feature appears blue when viewed in transmitted light and metallic yellow when viewed in incident light, the method comprising the steps of: A) printing a UV-Vis radiation curable security ink according to any one of claims 1 to 12 on a transparent or partially transparent area of ​​a substrate of a value document to provide an ink layer; and B) UV-Vis curing of the ink layer obtained in step A) to form a security feature.

14. The method according to claim 13, wherein the UV-Vis radiation curable security ink according to any one of claims 1 to 12 is printed on a transparent or partially transparent area of ​​a substrate of a value document by screen printing, rotogravure printing, or flexographic printing to provide an ink layer.

15. The method according to claim 13 or 14, wherein the valuable document is selected from banknotes, contracts, bills, checks, vouchers, tax stamps, agreements, identity documents, passes, cards, academic diplomas, and degrees.