A kind of battery sludge porous Ni / Co / Li ozone catalyst and preparation method thereof
The porous Ni/Co/Li ozone catalyst is prepared through drying, crushing, balling, drying and roasting processes, which solves the problem of unutilized resources and high cost in battery sludge treatment, improves catalytic performance and COD removal rate, and achieves The harmlessness and resource utilization of battery sludge reduces production costs.
Patent Information
- Application Number
- CN202310496162.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2022-05-06
- Filing Date
- 2023-05-05
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2043-05-05
AI Technical Summary
Existing battery sludge treatment methods have problems such as unused resources, environmental pollution and high costs. In particular, the solidification and recycling efficiency of heavy metal sludge is low, and traditional methods consume a lot of energy and chemical reagents, resulting in secondary pollution and high production. cost.
The porous Ni/Co/Li ozone catalyst is prepared by drying, crushing, balling, drying and roasting processes. Through far-infrared drying, crushing, mixing, shaping and roasting steps, Ni, Co, Li and other metals in battery sludge are utilized. , forming an efficient ozone catalyst, increasing the specific surface area and pore volume of the catalyst, and improving the catalytic performance.
It achieves the harmlessness and resource utilization of battery sludge, significantly improves the catalytic performance of the ozone catalyst, increases the COD removal rate by 30%-50%, reduces the production cost by 60%-80%, extends the service life of the catalyst, and The circular economy concept of "using waste to make waste" has been realized.
Abstract
Description
Technical Field
[0001] The invention relates to a battery sludge porous Ni / Co / Li ozone catalyst and a preparation method thereof, and in particular to a battery sludge treatment method and an ozone catalyst and a preparation method thereof which have the advantages of simple preparation process, environmental friendliness, strong controllability in operation and economic feasibility. Background Art
[0002] With the rapid development of economy and industry in recent years, more heavy metal sludge has been produced in the battery, electric lock, electronics, hardware, chemical, smelting and other industries. Heavy metal sludge contains copper, zinc, chromium, nickel, cobalt, lithium, etc., and NaClO, Na 2 S, FeSO 4 , NaOH, Ca(OH) 2 Therefore, the sludge contains not only various heavy metals, but also other chemical salts, surfactants, etc. The composition is very complex and it is a hazardous waste.
[0003] Heavy metal pollutants in battery sludge seriously threaten environmental safety, mainly manifested in the following aspects: ① Heavy metal sludge occupies large areas of land, causing soil pollution. ② Some heavy metal ions in heavy metal sludge will dissolve into water bodies, causing water pollution. Entering the human body through the environment or food chain, it poses a huge threat to human health. ③ Heavy metal sludge generates toxic and harmful gases, further polluting the air and environment.
[0004] Regarding the treatment methods of battery sludge, at present, the treatment of industrial sludge containing heavy metals at home and abroad mainly includes solidification / stabilization technology, thermal treatment technology of heavy metal sludge and heavy metal sludge recycling technology.
[0005] Solidification / stabilization technology solidifies and stabilizes heavy metals in sludge, but heavy metals are not recovered and resource utilization cannot be achieved. Thermochemical treatment consumes a lot of energy and increases treatment costs. Acid leaching, ammonia leaching and biological leaching use a large amount of chemical reagents, which increases costs and may cause secondary pollution. The acid leaching method has a good effect on removing heavy metals from sludge and takes a short time, but it requires a large amount of acid. According to statistics, the mass ratio of acid to dry sludge is 0.5-0.8, the cost of acid consumption is 220.48 yuan per ton of dry sludge, and the lime consumption for neutralizing the acid in the leaching liquid is 176.40 yuan per ton of dry sludge, and the residual sludge still needs to be treated.
[0006] Among the main components of the sludge from battery production wastewater treatment, water accounts for 50%-70%, cobalt accounts for 1%-30%, Li accounts for 2%-3%, nickel accounts for 3%-4%, calcium, silicon, and iron account for 8%-10%, and carbon accounts for 5%-10%. The metals contained in it, such as Co, Ni, Fe, and Li, are the effective components of ozone catalysis. From the perspective of sludge treatment and disposal, with battery sludge as the main component, an efficient, environmentally friendly, and economical ozone catalyst has been developed, which can make full use of the metals Ni, Co, Li, and Cr in the battery sludge to realize the resource utilization and harmlessness of the battery sludge.
[0007] The present invention combines the characteristics of battery sludge and selects dehydration, crushing, pelletizing, drying and roasting processes to prepare porous Ni / Co / Li ozone catalyst, thereby achieving harmlessness of battery sludge and simultaneous resource utilization of effective components. Summary of the invention
[0008] One of the purposes of the present invention is to provide a method for preparing a porous Ni / Co / Li ozone catalyst from battery sludge and its application. The method has simple process, no pollution and strong controllability in operation.
[0009] To achieve the above-mentioned purpose, the present invention provides a method for preparing an ozone catalyst, using battery sludge, and adopting drying and dehydration, crushing, conditioning and mixing, pelletizing, drying, roasting, and cooling processes to prepare a porous Ni / Co / Li ozone catalyst, comprising the following steps:
[0010] ① Dry the battery sludge to be treated by far infrared drying at 110℃-130℃ for 50-80min to obtain dry sludge;
[0011] ② Crushing the dry sludge into active catalytic powder in the crusher;
[0012] ③ Evenly mix the active catalytic powder, pore-forming agent powder and catalytic conditioner powder obtained in ② to form a catalytic mixture powder. Start the pelletizing machine, spray the binder to form catalyst raw material balls, dry, roast and cool the obtained catalyst raw material balls to obtain porous Ni / Co / Li ozone catalyst;
[0013] For further improvement, the weight proportions of the active catalytic powder, pore former powder and catalytic conditioner powder in the catalytic mixture are 87.5%-94.0%, 1.0%-4.5% and 5.0%-8.0% respectively.
[0014] For further improvement, the particle size of the active catalytic powder is in the range of 80-100 mesh.
[0015] For further improvement, the pore-forming agent powder can be selected from any one of hydroxypropyl cellulose, polyethylene glycol, and polyvinyl alcohol, or multiple components can be mixed and used, with a particle size of 80-100 meshes.
[0016] For further improvement, the catalyst conditioner powder can be selected from any one of the metals or metal oxides such as Cu, Sn, Mn, etc., or multiple components can be mixed and used, with a particle size of 80-100 mesh.
[0017] For further improvement, the main adhesive is boric acid, and the auxiliary adhesive can be selected from water glass, aluminum sol, and water, or multiple components can be mixed and added in a certain proportion. The main adhesive and the auxiliary adhesive are in a mass ratio of 1:2-1:5, and the two are mixed into an adhesive before use.
[0018] For further improvement, the catalytic mixture powder and the binder are in a mass ratio of 9:1-19:1.
[0019] For further improvement, the catalyst molded raw material balls are dried at a temperature of 110-130° C. for 2 h-3 h.
[0020] For further improvement, the catalyst formed raw material balls are calcined at a high temperature of 600°C-900°C for 3-6 hours.
[0021] The second object of the present invention is to provide an ozone catalyst prepared by any of the preparation methods in the aforementioned experimental methods, and its raw material is heavy metal battery sludge containing Ni, Co, Li and other active metals and metal oxides.
[0022] The third object of the present invention is to provide the application of the ozone catalyst in the above test method in the process of treating organic wastewater.
[0023] The present invention has the following beneficial effects: the porous Ni / Co / Li ozone catalyst provided by the invention is prepared by using effective catalytic elements such as Ni, Co, and Li in battery sludge, the catalyst body is full of active substances, the active components are not easy to lose, the service life is 5-10 years, and the raw materials are easy to obtain, which reduces the production cost of the catalyst. In addition, the catalytic active components are evenly distributed. When preparing the catalyst, a pore-forming agent is appropriately added to increase the specific surface area and pore volume of the catalyst, which is conducive to the full contact between the catalyst and ozone and pollutants, and significantly improves the catalytic performance of the catalyst. Compared with ozone catalysts prepared by other methods, the wastewater COD removal rate is increased by 30%-50%, the production cost is reduced by 60%-80%, and the battery sludge is fully utilized, realizing the concept of waste treatment. DETAILED DESCRIPTION
[0024] Based on the two invention purposes of saving battery sludge treatment costs and improving the effect of ozone catalysts, the present invention provides a battery sludge porous Ni / Co / Li ozone catalyst and a preparation method thereof, and the preparation method comprises the following steps:
[0025] The battery sludge to be treated is dried by far infrared drying at 110℃-130℃ for 50-80min to obtain dry sludge. The dry sludge is crushed by a crusher to obtain active catalytic powder. The active catalytic powder, pore-forming agent powder and catalytic conditioner powder are mixed evenly to obtain catalytic mixture powder, and the ball forming machine is started to spray the binder to form catalyst raw material balls. The obtained catalyst raw material balls are dried and calcined to obtain porous Ni / Co / Li ozone catalyst.
[0026] The weight proportions of active catalytic powder, pore former powder and catalytic conditioner powder in the catalytic mixture powder are 87.5%-94.0%, 1.0%-4.5% and 5.0%-8.0% respectively.
[0027] The catalytic mixture powder has a high content of oxides of metals such as Ni, Co, and Li. The oxide of battery sludge is used as a catalyst, and the catalyst is dehydrated, pelletized, dried, and calcined at one time. The structure of the catalyst is firm and stable compared to the supported catalyst, and the active components are not easy to lose. At the same time, the active components in the sludge that can be used for ozone catalysis are effectively utilized, reducing the production cost of the catalyst.
[0028] The main active components in the battery sludge are oxides of metals such as Ni, Co, and Li. The above-mentioned catalyst powder provides active sites for ozone catalysis and accelerates the reaction rate of ozone oxidation. The particle size of the powder is in the range of 80-100 mesh. When preparing the ozone catalyst, the proportion of active catalytic powder, pore former, and catalytic conditioner powder can be selected according to actual needs. Battery sludge with different metal oxide contents can also be blended to achieve the best ozone catalytic effect.
[0029] The pore-forming agent is added to form pores in the ozone catalyst, increase its specific surface area and pore volume, better exert the catalytic effect of the active substances in the battery sludge, and enhance the catalytic performance. The particle size of the pore-forming agent is selected to be 80-100 mesh. The pore-forming agent can be selected from any one of hydroxypropyl cellulose, polyethylene glycol, and polyvinyl alcohol, or multiple components can be mixed and used. The amount of pore-forming agent added should be appropriate. When the amount of pore-forming agent added is too high, the pores of the catalyst spheres are large, and the strength is insufficient, and it is easy to break during operation. When the added content of the pore-forming agent is low, the voids are few and small, and the ozone catalytic effect is not good.
[0030] The binder plays the role of bonding the powder and wetting the powder when the catalytic mixture is formed into raw material balls. The binder includes a main binder and an auxiliary binder. The main binder is boric acid, and the auxiliary binder can be selected from water glass, aluminum sol, and water, or multiple components can be mixed and added in a certain proportion. The main binder and the auxiliary binder are mixed in a mass ratio of 1:2-1:5 before use, so that the concentration of the binder is appropriate, the reaction speed is fast during the bonding and forming process, and the strength of the balls is high and not easy to break.
[0031] The catalyst conditioner plays a role in improving the catalytic performance of the ozone catalyst. The main component is a mixture of any one or more of metals or metal oxides such as Cu, Sn, and Mn, and the particle size is within the range of 80-100 mesh.
[0032] The amount should be appropriate. Too much will destroy the economic efficiency of making ozone catalysts, and too little will affect the ozone catalytic effect due to too little active substances in the battery sludge.
[0033] In the process of forming the catalytic mixture powder into spheres, the mass ratio of the added amount of the catalytic mixture powder and the binder is 19:1-9:1, and the particle size of the spheres is controlled to be 3mm-5mm. The amount of binder added is preferably within this range. Adding too much or too little binder will affect the catalyst sphere forming effect.
[0034] After integrating various ozone catalyst preparation methods and multiple blending experiments, the weight ratios of active catalytic powder, pore-forming agent powder, and catalytic conditioner powder were obtained: 87.5%-94.0%, 1.0%-4.5%, and 5.0%-8.0%, respectively. The ozone catalytic effect is good, the spheres are firm, and the contact area between the catalyst and the sewage to be treated is large.
[0035] The formed raw material balls are dried at 110-130°C for 2h-3h, and then calcined at 600-900°C for 3-6 hours to form a solid ozone catalyst. The chemical adhesive used in the preparation process increases the strength of the catalyst during the molding process and extends the service life of the catalyst.
[0036] In addition, through the above production steps and production parameters, the present invention provides a battery sludge Ni / Co / Li ozone catalyst, the raw material of which is heavy metal battery sludge containing Ni, Co, Li and other active metals and metal oxides.
[0037] The following will combine specific examples to compare the performance of the ozone catalyst provided by the present invention with that obtained by other preparation methods, and then analyze the feasibility of using battery sludge as an ozone catalyst from an economic perspective;
[0038] Embodiment 1.
[0039] The moisture content of the battery sludge to be treated is 75%. The battery sludge to be treated is dried by far infrared drying at 130°C for 60 minutes. At this time, the moisture content of the battery sludge is 15%. The dehydrated and dried dry sludge is crushed by a crusher to obtain active catalytic powder with a particle size between 80-100 meshes. The Co content in the sludge powder is 57.45% and the Li content is 6.56%.
[0040] Take polyvinyl alcohol powder and Cu powder with a particle size of 80-100 mesh, and mix the active catalytic powder, polyvinyl alcohol powder and copper powder in a mass fraction of 91%:3%:6%.
[0041] The above catalytic mixture is placed in a pelletizing machine, and a binder with a ratio of 4:1 of water and boric acid is sprayed in, and the amount of binder added is 9% of the mass of the catalytic mixture. The binder is first mixed evenly, then sprayed, and then rolled into balls to prepare catalyst raw material balls with a particle size of 3mm-5mm.
[0042] The raw material balls are dried at 120°C for 3 hours and calcined in a high-temperature furnace at 700°C for 5 hours to obtain the desired porous Ni / Co / Li ozone catalyst product.
[0043] This embodiment is realized by comparing ozone catalysts prepared by different methods as follows: three ozone oxidation reactors with the same specifications and effective volume of 250L are filled with impregnation roasting ozone catalysts (loaded with Mn and Fe oxides), ordinary γ-Al 2 O 3 Catalyst, and the porous Ni / Co / Li ozone catalyst in this embodiment. The printing and dyeing wastewater was deeply treated under the following process conditions: ozone dosage of 40 mg / L, hydraulic retention time of 65 min. The treatment results of the three catalysts are as follows:
[0044] Ordinary γ-Al 2 O 3 The catalyst treated the influent with COD of 212 mg / L, the effluent COD was 130 mg / L, and the COD removal rate was 38.68%; the impregnation roasting ozone catalyst treated the influent with COD of 198 mg / L, the effluent COD was 50 mg / L, and the COD removal rate was 74.74%; the porous Ni / Co / Li ozone catalyst in Example 1 treated the influent with COD of 206 mg / L, the effluent COD was 56 mg / L, and the COD removal rate was 72.82%.
[0045] From the treatment results of the ozone catalyst, it can be seen that under the same conditions, the catalytic effect of the ozone catalyst in Example 1 is far better than that of adding ordinary γ-Al 2 O 3The catalytic effect is basically the same as that of the ozone catalyst prepared by the impregnation method;
[0046] Embodiment 2.
[0047] The moisture content of the battery sludge to be treated is 79%. The battery sludge to be treated is dried by far infrared drying at 130°C for 55 minutes. At this time, the moisture content of the battery sludge is 17%. The dehydrated and dried dry sludge is crushed by a crusher to obtain active catalytic powder with a particle size between 80-100 meshes. The Co content of the sludge powder is 0.76%, the Li content is 1.69%, and the Ni content is 3.41%.
[0048] Take polyethylene glycol powder and Mn powder with a particle size of 80-100 mesh separately, and mix the active catalytic powder, polyethylene glycol powder and manganese powder in a mass fraction of 90%:3.5%:6.5%.
[0049] The above catalytic mixture is placed in a pelletizing machine, and a binder of water and boric acid in a ratio of 2:1 is sprayed in, and the binder addition amount is 9% of the mass of the catalytic mixture. The binder is first mixed evenly, then sprayed, and then rolled into balls to prepare catalyst raw material balls with a particle size of 3mm-5mm.
[0050] The catalyst raw material balls are dried at 120°C for 3 hours and calcined in a high-temperature furnace at 700°C for 5 hours to obtain the required ozone catalyst product.
[0051] This embodiment is realized by comparing the ozone catalysts prepared by the following different methods: three ozone oxidation reactors with the same specifications and an effective volume of 250L were filled with the same mass and particle size of the impregnation roasting ozone catalyst (loaded with Mn and Ni oxides), the common γ-Al 2 O 3 Catalyst, and the ozone catalyst in this embodiment.
[0052] The process conditions for deep treatment of industrial high-salinity wastewater are: ozone dosage of 50 mg / L, hydraulic retention time of 55 min. The treatment results of the three catalysts are as follows:
[0053] Ordinary γ-Al 2 O 3 The catalyst treated the influent with COD of 124 mg / L, the effluent COD was 80 mg / L, and the COD removal rate was 35.48%; the impregnation roasting ozone catalyst treated the influent with COD of 117 mg / L, the effluent COD was 35 mg / L, and the COD removal rate was 70.00%; the porous Ni / Co / Li ozone catalyst in Example 2 treated the influent with COD of 129 mg / L, the effluent COD was 40 mg / L, and the COD removal rate was 68.99%.
[0054] From the treatment results of the ozone catalyst, it can be seen that under the same conditions, the catalytic effect of the ozone catalyst in Example 2 is far better than that of adding ordinary γ-Al 2 O 3 The catalytic effect is basically the same as that of the ozone catalyst prepared by the impregnation method;
[0055] Embodiment three.
[0056] The moisture content of the battery sludge to be treated is 72%. The battery sludge to be treated is dried by far infrared drying at 130°C for 60 minutes. At this time, the moisture content of the battery sludge is 20%. The dehydrated and dried sludge is crushed by a crusher. After crushing, the particle size of the active catalytic powder is between 80-100 meshes. The Co content in the sludge powder is 5.42%, the Li content is 7.66%, and the Ni content is 1.63%.
[0057] Take hydroxypropyl cellulose powder and Mn powder with a particle size of 80-100 mesh, and blend the battery sludge dried powder, hydroxypropyl cellulose powder and manganese powder in a mass fraction of 89%:3.5%:7.5%.
[0058] The above blended catalytic mixture is placed in a ball forming machine, and a binder with a ratio of 2.5:1 of water and boric acid is sprayed in, and the amount of binder added is 9% of the mass of the catalytic mixture. The binder is first mixed evenly, then sprayed, and then rolled into balls to prepare catalyst raw material balls with a particle size of 3mm-5mm.
[0059] The catalyst raw material pellets were dried at 115°C for 3 hours and calcined in a high-temperature furnace at 750°C for 5 hours to obtain the desired ozone catalyst product.
[0060] This embodiment is realized by comparing ozone catalysts prepared by different methods as follows: three ozone oxidation reactors with the same specifications and an effective volume of 250L are filled with impregnation and roasting ozone catalysts (γ-Al loaded with Cr, Ni and Li) of the same mass and particle size. 2 O 3 catalyst), and the ozone catalyst in this embodiment.
[0061] The coking wastewater was deeply treated under the following process conditions: ozone dosage was 60mg / L, hydraulic retention time was 60min. The treatment results of the three catalysts are as follows:
[0062] Ordinary γ-Al 2 O 3The catalyst treated the influent with a COD of 303 mg / L, the effluent COD was 190 mg / L, and the COD removal rate was 37.29%; the impregnation roasting ozone catalyst treated the influent with a COD of 312 mg / L, the effluent COD was 70 mg / L, and the COD removal rate was 77.56%; the porous Ni / Co / Li ozone catalyst in Example 2 treated the influent with a COD of 319 mg / L, the effluent COD was 76 mg / L, and the COD removal rate was 76.17%.
[0063] From the treatment results of the ozone catalyst, it can be seen that under the same conditions, the catalytic effect of the ozone catalyst in Example 3 is far better than the catalytic effect of adding ordinary γ-Al2O3, and is basically the same as the effect of the ozone catalyst prepared by the impregnation method.
[0064] From the above three examples, it can be seen that the catalytic effects of the ozone catalyst prepared by the impregnation method and the ozone catalyst made by recycling battery sludge are similar. Now the two methods are analyzed from an economic perspective.
[0065] Economically, battery sludge is treated as hazardous waste because it contains heavy metals. Generally, the cost of hazardous waste treatment varies depending on the sludge disposal process used. However, converting battery sludge into ozone catalyst can save the cost of hazardous waste treatment.
[0066] An economic analysis was conducted on the ozone catalyst preparation process. In the examples of the present invention, the treatment effect of this process is not much different from that of the ozone catalyst prepared by the impregnation method. During the preparation process, the impregnation method requires the purchase of heavy metal salts used in the impregnation solution, while the method of the present invention makes full use of the heavy metal salts in the battery sludge, saving the cost of heavy metal salts.
[0067] An economic analysis was conducted in the treatment process of battery sludge. The treatment of industrial sludge containing heavy metals mainly includes solidification / stabilization technology, thermal treatment technology of heavy metal sludge and heavy metal sludge recycling technology. Solidification / stabilization technology solidifies and stabilizes heavy metals in sludge, but does not recover heavy metals and cannot achieve resource utilization. Thermochemical treatment consumes a lot of energy and increases treatment costs. Acid leaching, ammonia leaching and biological leaching use a lot of chemical reagents, which increases costs and may cause secondary pollution. Acid leaching is more effective in removing heavy metals from sludge and takes a shorter time, but it requires a lot of acid.
[0068] In summary, making full use of the effective metal components of battery sludge to develop a porous Ni / CO / Li composite ozone catalyst can achieve the harmlessness and resource utilization of battery sludge. At the same time, using the catalyst provided by the invention for wastewater treatment can realize the concept of "waste treatment" and circular economy, and can effectively solve the treatment of sludge in battery enterprises.
[0069] The above contents are further detailed descriptions of the present invention in combination with specific implementations, but do not mean that the specific implementations of the present invention are limited to these examples. For ordinary technicians in the technical field to which the present invention belongs, several simple deductions or substitutions can be made without departing from the concept of the present invention, which should be regarded as falling within the protection scope of the present invention.
Claims
1. A method for preparing a porous Ni-Co-Li ozone catalyst using battery sludge, characterized in that: The porous Ni-Co-Li ozone catalyst is prepared by using battery sludge through drying and dehydration, crushing, conditioning and mixing, pelletizing, drying, roasting and cooling processes, including the following steps: ① Dry the battery sludge to be treated by far infrared drying at 110℃-130℃ for 50-80min to obtain dry sludge; ② Crushing the dry sludge into active catalytic powder in the crusher; ③ The active catalytic powder, pore-forming agent powder and catalytic conditioner powder obtained in ② are mixed evenly to form a catalytic mixture powder, a pelletizing machine is started, and a binder is sprayed to form catalyst raw material balls, and the obtained catalyst raw material balls are dried, roasted and cooled to obtain a porous Ni-Co-Li ozone catalyst; The pore-forming agent powder is selected from any one of hydroxypropyl cellulose, polyethylene glycol, and polyvinyl alcohol or a mixture of multiple components, and the particle size is 80-100 meshes; The catalyst conditioner powder is selected from any one of Cu, Sn, Mn metal or metal oxide or a mixture of multiple components, with a particle size of 80-100 mesh; The weight proportions of the active catalytic powder, pore-forming agent powder, and catalytic conditioner powder are 87.5%-94.0%, 1.0%-4.5%, and 5.0%-8.0%, respectively; The battery sludge raw material is heavy metal battery sludge containing Ni, Co, Li and other active metals and metal oxides.
2. The preparation method according to claim 1, characterized in that The particle size of the active catalytic powder is in the range of 80-100 mesh.
3. The preparation method according to claim 1, characterized in that: The main adhesive is boric acid, and the auxiliary adhesive is any one or more of water glass, aluminum sol, and water mixed and added in a certain proportion. The main adhesive and the auxiliary adhesive are mixed in a mass ratio of 1:2-1:5 to form the adhesive described in step ③ for use.
4. The preparation method according to claim 1, characterized in that: The mass ratio of the catalytic mixture powder to the binder is 9:1-19:
1.
5. The preparation method according to claim 1, characterized in that: The catalyst formed raw material balls are dried at a temperature of 110-130° C. for 2 h-3 h.
6. The preparation method according to claim 1, characterized in that: The catalyst formed raw material balls are roasted at a high temperature of 600° C.-900° C. for 3-6 hours.