Nickel-molybdenum solid solution-molybdenum oxide composite catalyst for high-selectivity preparation of perfluoroalkyl alcohol, preparation method and application
Through the synergistic effect of nickel-molybdenum solid solution and molybdenum oxide composite catalyst, the problem of difficulty in hydrogenation of perfluoroalkyl acids at low temperatures is solved, and the preparation of perfluoroalkyl alcohols with high selectivity and high activity is achieved, which is suitable for industrial production. .
Patent Information
- Application Number
- CN202310372047.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-10
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2043-04-10
AI Technical Summary
It is difficult for existing catalysts to effectively catalyze the hydrogenation of perfluoroalkyl acids to form perfluoroalkyl alcohols at low temperatures, and the reaction conditions of non-precious metal catalysts are harsh and their activity is insufficient, which limits industrial applications.
The heterogeneous catalyst was prepared by impregnation method using the nickel-molybdenum solid solution and molybdenum oxide composite catalyst (Ni1-xMox)-MoOy/TiO2. The synergistic effect of NiMo solid solution and Mo6+, Mo5+, and Mo4+ mixed molybdenum oxides was used to improve catalytic activity and Selective.
It has achieved high selectivity and high activity hydrogenation conversion of perfluoroalkyl acids, high catalytic activity, selectivity exceeding 90%, mild conditions, suitable for industrial production, and high catalyst stability.
Smart Images

Figure CN116440919B_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the field of nanocatalysis, and relates to a solid solution-metal oxide composite catalyst, a preparation method and an application thereof, and specifically relates to a catalyst composited with a nickel-molybdenum solid solution and a molybdenum oxide and a preparation method thereof, and provides a method for preparing perfluoroalkyl alcohols from perfluoroalkyl acids with high selectivity at low temperatures. Background Art
[0002] Alcohols in which all hydrogen atoms in the carbon chain are replaced by fluorine are called perfluoroalkyl alcohols. Due to the presence of perfluorocarbon chains, perfluoroalkyl alcohols have unique chemical stability, corrosion resistance, flame retardancy, etc. They are widely used in surfactants, fabric finishing agents, pharmaceutical intermediates and other fields. They are also the main components of foam fire extinguishers. As the demand for perfluoroalkyl alcohols increases year by year and the market demand is vast, it is crucial to carry out production research on perfluoroalkyl alcohols. It is a feasible route to directly replace the hydrogen atoms in the corresponding hydrocarbon carboxylic acid molecules with fluorine atoms generated by electrolysis to generate perfluoroalkyl acids, and then hydrogenate and reduce the perfluoroalkyl acids to generate perfluoroalkyl alcohols.
[0003] Since the hydrogenation of perfluoroalkyl acids is difficult, the current research on perfluoroalkyl alcohols is mainly aimed at hydrogenating perfluoroalkyl esters to produce perfluoroalkyl alcohols. In 1967, Case et al. used copper oxide catalysts to catalyze the hydrogenation of methyl trifluoroacetate to produce trifluoroethanol (US Pat. Nos. 3,314,987). In the same year, Anello et al. used ruthenium and palladium catalysts to catalyze the hydrogenation of fluorinated esters to produce fluorinated alcohols (US Pat. No. 3,356,746).
[0004] However, it is more difficult to directly hydrogenate fluorinated alkyl acids into corresponding primary alcohols than esters. Smith used an in-situ generated Re black catalyst to catalyze the hydrogenation of trifluoroacetic acid and heptafluorobutyric acid into corresponding primary alcohols (The Journal of Organic Chemistry, 1959, 24 (12): 1847-1854). However, the reaction conditions are very harsh, with a hydrogen pressure of about 30 MPa, a temperature above 200°C, and a reaction time of 18.5 hours. Fischer used a ruthenium catalyst at high temperature and high pressure to hydrogenate perfluoroalkyl acids to produce corresponding alcohols (US Pat. No. 3,663,629). However, the reaction process requires the presence of an initial water system, which increases the difficulty of production. Novotny used a solid Rh or Ir catalyst, a temperature of 50-150°C, and a H2 pressure of 0.5-1.5 MPa to hydrogenate trifluoroacetic acid into trifluoroethanol (US Pat. Nos. 4,273,947).
[0005] Due to the difficulty of hydrogenating perfluoroalkyl acids, the catalysts currently used for catalytic hydrogenation of perfluoroalkyl acids to produce perfluoroalkyl alcohols are mainly precious metal catalysts, which are expensive and difficult to be widely used in industrialization; non-precious metal catalysts require harsh reaction conditions and their activity needs to be improved. Based on the above, this patent aims to utilize a solid solution-metal oxide composite catalyst with high hydrogenation activity, and with the synergistic effect of the two, improve the catalytic hydrogenation ability of the catalyst and realize the conversion of perfluoroalkyl acids at low temperatures. Summary of the invention
[0006] In view of the problems existing in the prior art, the present invention provides a solid solution-metal oxide composite catalyst for high-activity and high-selectivity hydrogenation of perfluoroalkyl acids to produce perfluoroalkyl alcohols, a preparation method and its application. The catalyst has high activity, selectivity and stability for catalyzing the hydrogenation of perfluoroalkyl acids (such as heptafluorobutyric acid, nonafluoropentanoic acid, pentafluorooctanoic acid, etc., but not limited to these) to produce corresponding alcohols.
[0007] In order to achieve the above object, the technical solution adopted by the present invention is:
[0008] A nickel-molybdenum solid solution-molybdenum oxide composite catalyst for high selectivity in preparing perfluoroalkyl alcohol from perfluoroalkyl acid, wherein the composite catalyst prepared by an impregnation method is a heterogeneous catalyst, and the specific composition is (Ni 1-x Mo x )-MoO y / TiO2 (x = 0 ~ 1, y = 2 ~ 3), the lattice constant of NiMo solid solution is The main characteristic peak of XRD is 44.4°~44.0°. The content of active components NiMo solid solution and molybdenum oxide is 5~20wt%, and the structure is spherical. The specific structure is NiMo solid solution with a particle size of 20~25nm and Mo with a particle size of 10~20nm. 6+ 、Mo 5+ 、Mo 4+ The mixed molybdenum oxide is loaded on the surface of the carrier TiO2 with a size of about 25nm.
[0009] A method for preparing a nickel-molybdenum solid solution and molybdenum oxide composite catalyst for preparing perfluoroalkyl alcohol from perfluoroalkyl acid with high selectivity, comprising the following steps:
[0010] (1) Nickel nitrate and ammonium heptamolybdate are dissolved in water at a molar ratio of 1:0.5-2, and stirred at 30-70° C. for 10-30 min to dissolve, wherein 1.48 g of nickel nitrate is added to every 3-10 mL of water, that is, the concentration of nickel nitrate is 1.7 mol / L-0.51 mol / L.
[0011] (2) Add titanium dioxide to the mixed solution obtained in step (1) at 30-50° C. and stir for 2-6 hours. In step (1), 0.2-0.7 g of titanium dioxide is added to every 3-10 mL of water. In this step, nickel nitrate and ammonium heptamolybdate are uniformly loaded onto the titanium dioxide.
[0012] (3) The mixed solution obtained in step (2) is transferred to a centrifuge tube, and centrifuged at 8000-10000 rpm for 10-20 min. The liquid phase after centrifugation is removed by decantation, and the obtained solid phase is dried at 70-150° C. for 6-15 h.
[0013] (4) After the dried sample obtained in step (3) is cooled to room temperature, it is ground into powder. The powder is calcined in a tube furnace at a temperature of 400 to 600° C. for 2 to 6 hours. In this step, the component NiMoO4 is generated, which promotes Mo to enter the Ni lattice.
[0014] (5) After the sample obtained in step (4) is cooled to room temperature, a mixed gas of 5% H2 and 95% N2 by volume is introduced into the tube furnace to reduce the high-valent metal in the sample. After heating to 500-700°C, maintain for 1-4 hours. The sample obtained after reduction is the corresponding (Ni 1-x Mo x )-MoO y / TiO2 catalyst. In this step, NiMoO4 is reduced to form NiMo solid solution and Mo 6+ 、Mo 5+ 、Mo 4+ Mixed molybdenum oxides.
[0015] Furthermore, the heating rate in step (4) and step (5) is 1 to 6°C / min;
[0016] Furthermore, the rate of introducing the mixed gas in step (5) is 20 to 100 mL / min. An application of a solid solution-metal oxide composite catalyst, which is applied to the selective preparation of perfluoroalkyl alcohol from perfluoroalkyl acid, and the specific implementation process of the catalytic reaction is: using a high-pressure reactor as a reaction vessel, (Ni 1-x Mo x )-MoO y / TiO2 catalyst, reaction substrate, and solvent are added to the reactor in sequence. After the reactor is sealed, 99.99% hydrogen is used as a reducing agent. The air in the reactor is first replaced with 1MPa hydrogen, and then the reactor is filled with hydrogen to 1-5MPa. The reaction is carried out at 70-130°C for 5-20 hours. 1-x Mo x )-MoO y / TiO2 catalyst, correspondingly add 1-5mmol reaction substrate (such as heptafluorobutyric acid, nonafluoropentanoic acid, 15fluorooctanoic acid, etc., but not limited to these), and 5-25mL solvent anhydrous ethanol.
[0017] The innovative point of the present invention is that the generated NiMo solid solution has better H2 adsorption capacity and can be combined with Mo 6+ 、Mo 5+ 、Mo 4+ The mixed molybdenum oxides produce a synergistic effect and better promote the reaction.
[0018] The beneficial effects of the present invention are:
[0019] (1) The present invention (Ni 1-x Mo x )-MoO y The / TiO2 catalyst has high catalytic activity in the process of catalyzing the reduction of perfluoroalkyl acid to produce perfluoroalkyl alcohol, and the catalytic perfluoroalkyl acid hydrogenation conversion rate is greater than 90%, and the selectivity is greater than 90%.
[0020] (2) The present invention (Ni 1-x Mo x )-MoO y / TiO2 is used as a catalyst for the hydrogenation reduction of perfluoroalkyl acids to produce perfluoroalkyl alcohols. The preparation process is simple, the conditions are mild, and the raw materials used are cheap and readily available, which is conducive to large-scale industrial production. The synthesized catalyst has high stability and can be stored in the environment for a long time. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 The solid solution-metal oxide composite catalyst (Ni 1-x Mo x )-MoO y / TEM image of TiO2;
[0022] Figure 2 The solid solution-metal oxide composite catalyst (Ni 1-x Mo x )-MoO y HRTEM image of / TiO2;
[0023] Figure 3 The solid solution-metal oxide composite catalyst (Ni 1-x Mo x )-MoO y / TiO2 and Ni / TiO2 XRD patterns. DETAILED DESCRIPTION
[0024] The present invention is further described in detail below in conjunction with implementation cases. Of course, the present invention is not limited to the following specific implementation cases.
[0025] Example 1
[0026] 1.48g of nickel nitrate hexahydrate and 0.21g of ammonium heptamolybdate were added to 7mL of deionized water and stirred at 70°C for 10min to dissolve. Subsequently, 0.4g of titanium dioxide was added to the above solution, and after continuing to stir and mix for 6h, the obtained mixed solution was transferred to a centrifuge tube, centrifuged at 8000rpm for 15min, the liquid phase after centrifugation was removed by pouring, and the obtained solid phase was dried at 150°C for 6h. After the dried sample was cooled to room temperature, it was ground into powder. Calcination was carried out in a tubular furnace, the calcination temperature was 500°C for 6h, and the heating rate was 1°C / min. After the obtained sample was cooled to room temperature, a mixed gas of 5% H2 and 95% N2 by volume was introduced into the tubular furnace to reduce the high-valent metals in the sample, the heating rate was 3°C / min, the rate of introducing the mixed gas was 100mL / min, and after heating to 500°C, it was maintained for 3h. The sample obtained after reduction is the corresponding (Ni 1-x Mo x )-MoO y / TiO2 catalyst.
[0027] The (Ni 1-x Mo x )-MoO y In the / TiO2 catalyst, the lattice constant of NiMo solid solution is The main characteristic peak of XRD is 44.4°. The content of active component NiMo solid solution is 10%, the content of molybdenum oxide is 5%, and the structure is spherical. The specific structure is NiMo solid solution with a particle size of 20nm and Mo with a particle size of 10nm. 6+ 、Mo 5+ 、Mo 4+ The mixed molybdenum oxide is loaded on the surface of the carrier TiO2 with a size of about 25nm.
[0028] Application of the catalyst in this example: 100 mg of the prepared (Ni 1-x Mo x )-MoO y / TiO2, 5mmol of 15-fluorooctanoic acid and 5mL of anhydrous ethanol were placed in an autoclave. 99.99% hydrogen was used as a reducing agent, and the air in the reactor was first replaced with 1MPa hydrogen, and then the reactor was filled with hydrogen to 3MPa, and the reaction was carried out at 130°C for 5h. The conversion rate of 15-fluorooctanoic acid was 95% and the selectivity of 15-fluorooctanol was 100% by GC, and the yield was 95%.
[0029] Example 2
[0030] 1.48g of nickel nitrate hexahydrate and 0.42g of ammonium heptamolybdate were added to 10mL of deionized water and stirred at 30°C for 20min to dissolve. Subsequently, 0.7g of titanium dioxide was added to the above solution, and after continuing to stir and mix for 2h, the obtained mixed solution was transferred to a centrifuge tube, centrifuged at 9000rpm for 20min, the liquid phase after centrifugation was removed by pouring, and the obtained solid phase was dried at 70°C for 12h. After the dried sample was cooled to room temperature, it was ground into powder. Calcination was carried out in a tubular furnace, the calcination temperature was 600°C for 2h, and the heating rate was 3°C / min. After the obtained sample was cooled to room temperature, a mixed gas of 5% H2 and 95% N2 was introduced into the tubular furnace to reduce the high-valent metals in the sample, the heating rate was 6°C / min, the rate of introducing the mixed gas was 20mL / min, and after heating to 600°C, it was maintained for 4h. The sample obtained after reduction is the corresponding (Ni 1-x Mo x )-MoO y / TiO2 catalyst.
[0031] The (Ni 1-x Mo x )-MoO y In the / TiO2 catalyst, the lattice constant of NiMo solid solution is The main characteristic peak of XRD is 44.0°. The content of active component NiMo solid solution is 10%, the content of molybdenum oxide is 10%, and the structure is spherical. The specific structure is NiMo solid solution with a particle size of 25nm and Mo with a particle size of 15nm. 6+ 、Mo 5 + 、Mo 4+ The mixed molybdenum oxide is loaded on the surface of the carrier TiO2 with a size of about 25nm.
[0032] Application of the catalyst in this example: 100 mg of the prepared (Ni 1-x Mo x )-MoO y / TiO2, 1mmol heptafluorobutyric acid and 5mL anhydrous ethanol were placed in an autoclave. 99.99% hydrogen was used as a reducing agent, and the air in the reactor was first replaced with 1MPa hydrogen, and then the reactor was filled with hydrogen to 5MPa, and the reaction was carried out at 70°C for 13h. The conversion rate of heptafluorobutyric acid was 42% and the selectivity of heptafluorobutanol was 100% and the yield was 42% as detected by GC.
[0033] Example 3
[0034] 1.48g of nickel nitrate and 0.84g of ammonium heptamolybdate were added to 3mL of deionized water and stirred at 50°C for 30min to dissolve. Subsequently, 0.2g of titanium dioxide was added to the above solution, and after continuing to stir and mix for 4h, the obtained mixed solution was transferred to a centrifuge tube, centrifuged at 10000rpm for 10min, the liquid phase after centrifugation was removed by pouring out, and the obtained solid phase was dried at 120°C for 15h. After the dried sample was cooled to room temperature, it was ground into powder. Calcination was carried out in a tubular furnace, the calcination temperature was 400°C for 4h, and the heating rate was 6°C / min. After the obtained sample was cooled to room temperature, a mixed gas of 5% H2 and 95% N2 was introduced into the tubular furnace to reduce the high-valent metals in the sample, the heating rate was 1°C / min, the rate of introducing the mixed gas was 60mL / min, and after heating to 700°C, it was maintained for 1h. The sample obtained after reduction is the corresponding (Ni 1-x Mo x )-MoO y / TiO2 catalyst.
[0035] The (Ni 1-x Mo x )-MoO y In the / TiO2 catalyst, the lattice constant of NiMo solid solution is The main characteristic peak of XRD is 44.0°. The content of active component NiMo solid solution is 10%, the content of molybdenum oxide is 20%, and the structure is spherical. The specific structure is NiMo solid solution with a particle size of 25nm and Mo with a particle size of 20nm. 6+ 、Mo 5 + 、Mo 4+ The mixed molybdenum oxide is loaded on the surface of the carrier TiO2 with a size of about 25nm.
[0036] Application of the catalyst in this example: 100 mg of the prepared (Ni 1-x Mo x )-MoO y / TiO2, 3mmol nonafluorooctanoic acid and 25mL anhydrous ethanol were placed in an autoclave. 99.99% hydrogen was used as a reducing agent, and the air in the reactor was first replaced with 1MPa hydrogen, and then the reactor was filled with hydrogen to 1MPa, and the reaction was carried out at 100°C for 20h. The GC detection showed that the conversion rate of nonafluoropentanoic acid was 83%, the selectivity of nonafluoropentanol was 95%, and the yield was 78.9%.
[0037] Example 4
[0038] 1.48g of nickel nitrate and 0.42g of ammonium heptamolybdate were added to 3mL of deionized water and stirred at 35°C for 10min to dissolve. Subsequently, 0.4g of titanium dioxide was added to the above solution, and after continuing to stir and mix for 4h, the obtained mixed solution was transferred to a centrifuge tube, centrifuged at 10000rpm for 10min, the liquid phase after centrifugation was removed by pouring out, and the obtained solid phase was dried at 100°C for 12h. After the dried sample was cooled to room temperature, it was ground into powder. Calcination was carried out in a tubular furnace, the calcination temperature was 550°C for 4h, and the heating rate was 2°C / min. After the obtained sample was cooled to room temperature, a mixed gas of 5% H2 and 95% N2 was introduced into the tubular furnace to reduce the high-valent metals in the sample, the heating rate was 2°C / min, the rate of introducing the mixed gas was 60mL / min, and after heating to 600°C, it was maintained for 2h. The sample obtained after reduction is the corresponding (Ni 1-x Mo x )-MoO y / TiO2 catalyst.
[0039] The (Ni 1-x Mo x )-MoO y / TiO2 catalyst morphology as shown in the attached Figure 1 As shown in the figure, the specific structure is a NiMo solid solution with a particle size of 25nm and a Mo particle size of 15nm. 6+ 、Mo 5+ 、Mo 4+ The mixed molybdenum oxide is loaded on the surface of the carrier TiO2 with a size of about 25nm. 1-x Mo x )-MoO y The lattice fringes of NiMo solid solution in / TiO2 catalyst have been found in the catalyst, such as the attached Figure 2 As shown, its lattice constant is (Ni 1-x Mo x )-MoO y The characteristic peak of NiMo solid solution in / TiO2 catalyst has a certain degree of deviation compared with single Ni. Figure 3 As shown, its main characteristic peak is 44.0°. The content of NiMo solid solution, an active component, in the catalyst is 10%, and the content of molybdenum oxide is 10%.
[0040] Application of the catalyst in this example: 100 mg of the prepared (Ni 1-x Mo x )-MoO y / TiO2, 1mmol nonafluoropentanoic acid and 10mL anhydrous ethanol were placed in an autoclave. 99.99% hydrogen was used as a reducing agent, and the air in the reactor was first replaced with 1MPa hydrogen, and then the reactor was filled with hydrogen to 3MPa, and the reaction was carried out at 120°C for 6h. The GC detection showed that the conversion rate of nonafluoropentanoic acid was 95%, the selectivity of nonafluoropentanol was 96%, and the yield was 91.2%.
[0041] Example 5
[0042] 1.48g of nickel nitrate hexahydrate and 0.315g of ammonium heptamolybdate were added to 10mL of deionized water and stirred at 50°C for 20min to dissolve. Subsequently, 0.7g of titanium dioxide was added to the above solution, and after continuing to stir and mix for 2h, the obtained mixed solution was transferred to a centrifuge tube, centrifuged at 9000rpm for 15min, the liquid phase after centrifugation was removed by pouring, and the obtained solid phase was dried at 150°C for 6h. After the dried sample was cooled to room temperature, it was ground into powder. Calcination was carried out in a tubular furnace, the calcination temperature was 530°C for 4h, and the heating rate was 5°C / min. After the obtained sample was cooled to room temperature, a mixed gas of 5% H2 and 95% N2 was introduced into the tubular furnace to reduce the high-valent metals in the sample, the heating rate was 2°C / min, the rate of introducing the mixed gas was 20mL / min, and after heating to 570°C, it was maintained for 4h. The sample obtained after reduction is the corresponding (Ni 1-x Mo x )-MoO y / TiO2 catalyst.
[0043] The (Ni 1-x Mo x )-MoO y In the / TiO2 catalyst, the lattice constant of NiMo solid solution is The main characteristic peak of XRD is 44.2°. The content of active component NiMo solid solution is 10%, the content of molybdenum oxide is 8%, and the structure is spherical. The specific structure is NiMo solid solution with a particle size of 23nm and Mo with a particle size of 13nm. 6+ 、Mo 5+ 、Mo 4+ The mixed molybdenum oxide is loaded on the surface of the carrier TiO2 with a size of about 25nm.
[0044] Application of the catalyst in this example: 100 mg of the prepared (Ni 1-x Mo x )-MoO y / TiO2, 2mmol heptafluorobutyric acid and 5mL anhydrous ethanol were placed in an autoclave. 99.99% hydrogen was used as a reducing agent, and the air in the reactor was first replaced with 1MPa hydrogen, and then the reactor was filled with hydrogen to 2MPa, and the reaction was carried out at 100°C for 8h. The conversion rate of heptafluorobutyric acid was 92%, the selectivity of heptafluorobutanol was 90%, and the yield was 82.8% as detected by GC.
[0045] It should be noted that the embodiments described above are only used to explain the present invention and do not constitute any limitation to the present invention. The present invention has been described with reference to typical embodiments, but it should be understood that the words used therein are descriptive and explanatory words, rather than restrictive words. The present invention may be modified as specified within the scope of the claims of the present invention, and the present invention may be revised without departing from the scope and spirit of the present invention. Although the present invention described therein relates to specific methods, materials and embodiments, it does not mean that the present invention is limited to the specific examples disclosed therein, on the contrary, the present invention can be extended to all other methods and applications with the same functions.
Claims
1. A method for preparing a nickel-molybdenum solid solution and molybdenum oxide composite catalyst for high selectivity of perfluoroalkyl acid to perfluoroalkyl alcohol, characterized in that: The following steps are involved: (1) dissolving nickel nitrate and ammonium heptamolybdate in water at a molar ratio of 1:0.5-2, stirring at 30-70° C. for 10-30 min to dissolve, wherein the concentration of nickel nitrate is 0.51 mol / L-1.7 mol / L; (2) adding titanium dioxide to the mixed solution obtained in step (1) at 30 to 50° C., stirring and mixing for 2 to 6 hours, and uniformly loading nickel nitrate and ammonium heptamolybdate onto the titanium dioxide; wherein, in step (1), 0.2 to 0.7 g of titanium dioxide is added to every 3 to 10 mL of water; (3) centrifuging the mixed solution obtained in step (2), removing the liquid phase, and drying the obtained solid phase; (4) After the dried sample obtained in step (3) is cooled to room temperature, it is ground into powder; calcined in a tube furnace at a temperature of 400 to 600° C. for 2 to 6 hours to generate a NiMoO4 component, which promotes Mo to enter the Ni lattice; (5) After the sample obtained in step (4) is cooled to room temperature, a mixed gas of H2 and N2 is introduced into the tube furnace to reduce the high-valent metal in the sample. After the temperature is raised to 500-700°C and maintained for 1-4 hours, NiMoO4 is reduced to generate NiMo solid solution and Mo 6+ 、Mo 5+ 、Mo 4+ Mix molybdenum oxide to obtain (Ni 1-x Mo x )-MoO y / TiO2 catalyst; the mixed gas includes 5% H2 and 95% N2 by volume; The composite catalyst is a heterogeneous catalyst, which is composed of (Ni 1-x Mo x )-MoO y / TiO2, wherein x=0-1, y=2-3, the structure is spherical, the content of the active components NiMo solid solution and molybdenum oxide is 5-20wt%, and the structure is NiMo solid solution with a particle size of 20-25nm and Mo with a particle size of 10-20nm 6+ 、Mo 5+ 、Mo 4+ The mixed molybdenum oxides are loaded on the surface of the carrier TiO2.
2. The preparation method according to claim 1, characterized in that: The centrifugal speed in step (3) is 8000-10000 rpm, and the centrifugal time is 10-20 min; the drying temperature is 70-150° C., and the time is 6-15 h.
3. The preparation method according to claim 1, characterized in that: The rate of introducing the mixed gas in the step (5) is 20 to 100 mL / min.
4. An application of a nickel-molybdenum solid solution-molybdenum oxide composite catalyst, characterized in that: The nickel-molybdenum solid solution-molybdenum oxide composite catalyst prepared by the preparation method described in any one of claims 1 to 3 is used to selectively prepare perfluoroalkyl alcohol from perfluoroalkyl acid, and the catalytic perfluoroalkyl acid hydrogenation conversion rate is greater than 90%, and the selectivity is greater than 90%.