A method for manufacturing mobile phone optical film

By using electrostatic film, PMMA/APET co-extruded lamination film and PET film composite in the mobile phone optical film, combined with nano-coating and enhanced coating, the problems of poor anti-fall, anti-corrosion and anti-radiation effects in the existing technology are solved. , improve production capacity and yield, extend service life, and reduce environmental pollution.

CN116442572BActive Publication Date: 2024-10-22SHENZHEN ZHONGYOU OPTICAL TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310228531.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-03-10
Publication Date
2024-10-22
Estimated Expiration
2043-03-10

AI Technical Summary

Technical Problem

Existing optical films for mobile phones have poor anti-fall, anti-corrosion, and anti-radiation effects, as well as low production capacity and low yield rates.

Method used

It uses a hardened layer, a primer layer, a silicone layer and a base material layer laminated in sequence from top to bottom. The base material layer is an electrostatic film. It is compounded with a PMMA/APET co-extruded laminating film and a PET film. The nano-coating has a discoloration effect. The coating liquid is sprayed on the surface of the tempered film with enhanced paint, combined with water-based peelable glue and optical functional resin, and hot pressed and UV cured to make a mobile phone optical film.

Benefits of technology

The anti-fall, anti-corrosion and anti-radiation properties are improved, the manufacturing cost is reduced, the yield is improved, the service life is extended, and environmental pollution is reduced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116442572B_ABST
    Figure CN116442572B_ABST
Patent Text Reader

Abstract

The invention discloses a method for manufacturing a mobile phone optical film, which belongs to the technical field of mobile phone films, and comprises a hardening layer, a primer layer, a silicone layer and a substrate layer which are sequentially stacked from top to bottom. The invention adopts a PMMA / APET co-extruded coating film and a PET film to compound the film, thereby enhancing the performances of anti-fall, anti-corrosion and anti-radiation. The PMMA / APET co-extruded coating film can achieve the softness requirement of the PMMA / APET co-extruded coating film by softening the film. The invention adopts a nano-coating method to coat a coating liquid with a color-changing effect on materials such as PET or OCA, and makes a layer of flexographic color on the coated side, a layer of UV transfer texture on the color-coated side, electroplating behind the texture, and roll-to-roll screen printing, thereby improving the production capacity and yield rate. An electrostatic film is used as a substrate, and a suitable thickness is selected. The curved screen protective film adapted to the curved screen is formed by film pressing, thereby effectively reducing the manufacturing cost, and effectively eliminating the difficulty of bubbling during the laminating process, thereby improving the yield rate.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of mobile phone diaphragms, in particular to a method for manufacturing a mobile phone optical diaphragm. Background Art

[0002] In recent years, mobile phone products have gradually entered the era of full-screen displays, and various manufacturers have also adopted various screen presentation methods. Mobile phone protective films are used to protect mobile phone screens and prevent scratches, bumps, etc. during use, thereby protecting the mobile phone screens. However, with the development of mobile phones, the existing mobile phone optical films have poor anti-drop, anti-corrosion, and anti-radiation effects, and there are also problems with low production capacity and low yield. Summary of the Invention

[0003] The purpose of the present invention is to provide a method for manufacturing a mobile phone optical film to solve the problems raised in the above background technology.

[0004] The technical solution of the present invention is: it includes a hardening layer, a primer layer, a silicone layer and a substrate layer stacked in sequence from top to bottom, the substrate layer is an electrostatic film, the thickness of the substrate layer is 25-100 μm, the thickness of the electrostatic film is 0.1 mm to 0.8 mm, the hardening layer, primer layer, silicone layer and substrate layer are made into a main film, PET film is provided on both sides of the main film, the main film also includes a PMMA / APET co-extruded coating film and a TPU film, the surface of the main film is coated with a reinforcing film, the surface of the substrate layer is provided with a water-based peelable glue, the surface of the substrate layer away from the water-based peelable glue is provided with an optical functional resin, the bottom surface of the silicone layer is provided with a heavy release film, an OCA anti-blue light material high viscosity layer is introduced on the silicone layer, a medium release film is provided on the OCA anti-blue light material high viscosity layer, and a coating liquid with a color-changing effect is coated on the PET film and the OCA anti-blue light material high viscosity layer;

[0005] The method for manufacturing the diaphragm further comprises the following steps:

[0006] Step 1: Slice the electrostatic film into uniform specifications;

[0007] Step 2: hot-press the sliced ​​electrostatic film at a temperature of 80°C to 90°C, apply glue or apply glue to the die-cut electrostatic film, and place a transparent adhesive layer around the outer edge of the electrostatic film. The peel strength of the adhesive layer is less than 20gf / inch, and the film is set aside.

[0008] Step 3: Apply water-based peelable glue on one side of the substrate layer and optical functional resin on the other side;

[0009] Step 4: Apply a coating liquid with a color-changing effect on the PET film by nano-coating;

[0010] Step 5: Apply a layer of flexo color on the coated side, and a layer of UV transfer texture on the coated side, and electroplate behind the texture;

[0011] Step 6: Take the coated substrate layer, apply a primer liquid on one side of the upper layer of the substrate layer, heat it in an oven to evaporate the solvent, and then perform UV curing to obtain a primer layer;

[0012] Step 7: After the first coating step is completed, a high-ductility hardening coating liquid is coated on the upper layer of the primer layer, and then heated in an oven to volatilize the solvent, and then UV-cured to obtain a high-ductility hardened layer;

[0013] Step 8: Soften the PMMA / APET co-extruded film by heating the PMMA / APET co-extruded film to 200-210° C. and keeping the temperature for 30 minutes, then cooling it to 100-120° C. and keeping the temperature for 30 minutes, and then cooling it to room temperature;

[0014] Step 9: Coating a polyurethane adhesive layer on one side of the softened PMMA / APET co-extruded film, and then laminating the side of the PET film coated with a silicone resin to both sides of the main film to form an integrated mobile phone screen protective film;

[0015] Step 10: spraying a reinforcing coating and an electrostatic film on the surface of the formed mobile phone screen protective film, and keeping the temperature at 110-120° C. for 5-7 hours to obtain a pre-treated tempered film;

[0016] Step 11: Keep the pretreated tempered film at a temperature of 150-160° C. for 3-5 hours to obtain an optical film.

[0017] Furthermore, the enhanced film is made by the following steps:

[0018] Step 1: Add styrene, hydroxyethyl methacrylate, azobisisobutylnitrile, and ethyl acetate to a reactor, stir and mix, then add 3-butylenetriethoxysilane to react, cool and add triethylamine to neutralize to obtain a first intermediate, add hydroxyethyl methacrylate, dodecafluoroheptyl methacrylate, isooctyl acrylate, styrene, azobisisobutylnitrile, and tetrahydrofuran to a reactor, and react together to obtain a second intermediate;

[0019] Step 2: Add the first intermediate, the second intermediate, toluene-3,5-diisocyanate, and N,N-dimethylformamide to a reactor, stir, and add dibutyltin dilaurate to react to obtain a third intermediate; add the third intermediate, methyltriethoxysilane, KH560, and xylene to a reactor, stir, add deionized water, adjust the pH value of the reaction solution, and react together to obtain a fourth intermediate;

[0020] Step 3: Add the fourth intermediate, antibacterial agent, potassium hydroxide, and N,N-dimethylformamide into the reactor to react to obtain a reinforcing liquid, mix the reinforcing liquid, nano-titanium dioxide, and defoaming agent evenly to obtain a reinforcing coating, and apply the reinforcing coating to form a reinforcing film.

[0021] Furthermore, in the first coating step, the base coat is coated by a micro-concave coating method, the rotation speed of the coating roller is 3 to 17 m / min, the feed speed of the substrate is 5 to 25 m / min, the oven temperature is 60 to 150°C, the curing time is 2 to 5 min, and the UV curing energy is 100 to 300 mJ / cm2. In the second coating step, the high ductility hardened layer (1) is coated by a micro-concave coating method, the rotation speed of the coating roller is 3 to 17 m / min, the feed speed of the substrate coated with the base coat (2) is 5 to 25 m / min, the oven temperature is 60 to 150°C, the curing time is 2 to 4 min, and the UV curing energy is 100 to 600 mJ / cm2.

[0022] Furthermore, the water-based peelable glue comprises water-based polyurethane emulsion, water-based acrylic emulsion release agent and water, and is coated by slit extrusion coating, gravure coating or screen printing coating.

[0023] Furthermore, the weight percentage of the aqueous polyurethane emulsion is between 19.5% and 60%, the weight percentage of the aqueous acrylic emulsion release agent is between 0.5% and 20%, and the weight percentage of water is between 20% and 80%.

[0024] Furthermore, the hardened layer comprises, by mass percentage, 30% to 45% of a polymer with hexafunctional unsaturated functional groups, 45% to 63% of a solvent, 2% to 8% of an initiator, and 1% to 5% of an additive; the primer layer comprises, by mass percentage, 20% to 55% of a polymer with trifunctional or tetrafunctional unsaturated functional groups, 40% to 75% of a solvent, and 2% to 8% of an initiator.

[0025] The present invention provides a method for manufacturing a mobile phone optical film through improvement, which has the following improvements and advantages compared with the prior art:

[0026] The present invention adopts PMMA / APET co-extruded coating film and PET film to compound, which enhances the performance of anti-fall, anti-corrosion and anti-radiation; the softness requirement of PMMA / APET co-extruded coating film can be achieved by softening the PMMA / APET co-extruded coating film, the present invention adopts nano-coating to apply a coating liquid with a color-changing effect on materials such as PET or OCA, and makes a layer of flexographic color on the coated side, and makes a layer of UV transfer texture on the coated side, electroplating behind the texture, and roll-to-roll screen printing, which is effective in improving production capacity and yield, and adopts electrostatic film as the substrate and selects a suitable thickness, through The curved screen protective film adapted to the curved screen is made by film pressing, which effectively reduces the manufacturing cost, and can effectively eliminate the difficulty of removing bubbles during the bonding process, thereby improving the yield rate. By spraying the enhanced coating, a hydrophobic and oleophobic layer can be formed on the surface of the tempered film, which can effectively prevent the adhesion of fingerprints or other stains. At the same time, the molecular side chain contains antibacterial ingredients, which can change the permeability of bacterial cell membranes and thus kill the cells. At the same time, the antibacterial effect of the mobile phone tempered film will not be greatly reduced due to long-term use, thereby increasing the service life of the mobile phone tempered film, improving the preparation efficiency of the optical film, and reducing the environmental pollution caused by the optical film during the preparation process. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] The present invention will be further explained below in conjunction with the accompanying drawings and Examples:

[0028] Figure 1 This is a schematic flow chart of a method for manufacturing a mobile phone optical film according to the present invention; DETAILED DESCRIPTION

[0029] The present invention will be described in detail below with reference to the accompanying drawings, clearly and completely describing the technical solutions in the embodiments of the present invention. Obviously, the embodiments described are only some embodiments of the present invention, not all embodiments. All other embodiments obtained by ordinary technicians in this field based on the embodiments of the present invention without making any creative efforts shall fall within the scope of protection of the present invention.

[0030] The present invention provides a method for manufacturing a mobile phone optical film through improvement. As shown in the figure, it includes a hardening layer, a primer layer, a silicone layer and a substrate layer stacked in sequence from top to bottom, the substrate layer is an electrostatic film, the substrate layer thickness is 25-100 μm, the electrostatic film thickness is 0.1 mm to 0.8 mm, the hardening layer, the primer layer, the silicone layer and the substrate layer are made into a main film, PET film is provided on both sides of the main film, the main film also includes a PMMA / APET co-extruded coating film and a TPU film, the main film surface is coated with a reinforcing film, the substrate layer surface is provided with a water-based peelable glue, the side of the substrate layer away from the water-based peelable glue is provided with an optical functional resin, the bottom surface of the silicone layer is provided with a heavy release film, an OCA anti-blue light material high viscosity layer is introduced on the silicone layer, a medium release film is provided on the OCA anti-blue light material high viscosity layer, and a coating liquid with a color-changing effect is coated on the PET film and the OCA anti-blue light material high viscosity layer;

[0031] The method for manufacturing the diaphragm further comprises the following steps:

[0032] Step 1: Slice the electrostatic film into uniform specifications;

[0033] Step 2: Hot-press the sliced ​​electrostatic film at a temperature of 80°C to 90°C, apply glue or apply glue to the die-cut electrostatic film, and place a transparent adhesive layer around the outer edge of the electrostatic film. The peel strength of the adhesive layer is less than 20gf / inch, and the film is set aside.

[0034] Step 3: Apply water-based peelable glue on one side of the substrate layer and optical functional resin on the other side;

[0035] Step 4: Apply a coating liquid with a color-changing effect on the PET film by nano-coating;

[0036] Step 5: Apply a layer of flexo color on the coated side, and a layer of UV transfer texture on the coated side, and electroplate behind the texture;

[0037] Step 6: Take the coated substrate layer, apply a primer liquid on one side of the upper layer of the substrate layer, heat it in an oven to evaporate the solvent, and then perform UV curing to obtain a primer layer;

[0038] Step 7: After the first coating step is completed, a high-ductility hardening coating liquid is coated on the upper layer of the primer layer, and then heated in an oven to volatilize the solvent, and then UV-cured to obtain a high-ductility hardened layer;

[0039] Step 8: Soften the PMMA / APET co-extruded film by heating the PMMA / APET co-extruded film to 200-210° C. and keeping the temperature for 30 minutes, then cooling it to 100-120° C. and keeping the temperature for 30 minutes, and then cooling it to room temperature;

[0040] Step 9: Coat one side of the softened PMMA / APET co-extruded film with a polyurethane adhesive layer, and then laminate the side of the PET film coated with the silicone resin to both sides of the main film to form an integrated mobile phone screen protective film;

[0041] Step 10: spraying a reinforcing coating and an electrostatic film on the surface of the formed mobile phone screen protective film, and keeping the temperature at 110-120° C. for 5-7 hours to obtain a pre-treated tempered film;

[0042] Step 11: Keep the pretreated tempered film at a temperature of 150-160° C. for 3-5 hours to obtain an optical film.

[0043] The enhanced membrane is made by the following steps:

[0044] Step 1: Add styrene, hydroxyethyl methacrylate, azobisisobutylnitrile, and ethyl acetate to a reactor, stir and mix, then add 3-butylenetriethoxysilane to react, cool and add triethylamine to neutralize to obtain a first intermediate, add hydroxyethyl methacrylate, dodecafluoroheptyl methacrylate, isooctyl acrylate, styrene, azobisisobutylnitrile, and tetrahydrofuran to a reactor, and react together to obtain a second intermediate;

[0045] Step 2: Add the first intermediate, the second intermediate, toluene-3,5-diisocyanate, and N,N-dimethylformamide to a reactor, stir, and add dibutyltin dilaurate to react to obtain a third intermediate; add the third intermediate, methyltriethoxysilane, KH560, and xylene to a reactor, stir, add deionized water, adjust the pH value of the reaction solution, and react together to obtain a fourth intermediate;

[0046] Step 3: Add the fourth intermediate, antibacterial agent, potassium hydroxide, and N,N-dimethylformamide into the reactor to react to obtain a reinforcing liquid, mix the reinforcing liquid, nano-titanium dioxide, and defoaming agent evenly to obtain a reinforcing coating, and apply the reinforcing coating to form a reinforcing film.

[0047] In the first coating step, the primer layer is coated by a micro-concave coating method, the rotation speed of the coating roller is 3 to 17 m / min, the feed speed of the substrate is 5 to 25 m / min, the oven temperature is 60 to 150°C, the curing time is 2 to 5 min, and the UV curing energy is 100 to 300 mJ / cm2. In the second coating step, the high ductility hardened layer (1) is coated by a micro-concave coating method, the rotation speed of the coating roller is 3 to 17 m / min, the feed speed of the substrate coated with the primer layer (2) is 5 to 25 m / min, the oven temperature is 60 to 150°C, the curing time is 2 to 4 min, and the UV curing energy is 100 to 600 mJ / cm2.

[0048] The water-based peelable glue includes a water-based polyurethane emulsion, a water-based acrylic emulsion release agent and water, and is coated by a slot extrusion coating method, a gravure coating method or a screen printing coating method.

[0049] The weight percentage of the waterborne polyurethane emulsion is between 19.5 and 60 percent, the weight percentage of the waterborne acrylic ester emulsion release agent is between 0.5 and 20 percent, and the weight percentage of water is between 20 and 80 percent.

[0050] The hardened layer includes, by weight percentage, 30% to 45% of a polymer with hexafunctional unsaturated functional groups, 45% to 63% of a solvent, 2% to 8% of an initiator, and 1% to 5% of an additive; the primer layer includes, by weight percentage, 20% to 55% of a polymer with trifunctional or tetrafunctional unsaturated functional groups, 40% to 75% of a solvent, and 2% to 8% of an initiator.

[0051] The electrostatic film is sliced ​​and cut into uniform specifications. The sliced ​​electrostatic film is hot-pressed at a temperature of 80°C to 90°C. The die-cut electrostatic film is glued or coated. A transparent adhesive layer is set around the outer edge of the electrostatic film. The peel strength of the adhesive layer is less than 20gf / inch and is kept aside. A water-based peelable glue is applied on one side of the substrate layer and an optical functional resin is provided on the other side. A coating liquid with a color-changing effect is applied on the PET film by nano-coating. A layer of flexographic color is applied on the coated side and a layer of UV transfer texture is applied on the colored side. The texture is electroplated behind the texture. The coated substrate layer is taken and a primer liquid is first applied on one side of the upper layer of the substrate layer. After heating in an oven and evaporating the solvent, UV curing is performed to obtain a primer layer. After completing the first coating step, a high-ductility hardening coating is applied on the upper layer of the primer layer. The mixture is heated in an oven to evaporate the solvent, and then UV cured to obtain a high ductility hardened layer. The PMMA / APET co-extruded laminated film is softened, and the PMMA / APET co-extruded laminated film is heated to 200-210°C and kept warm for 30 minutes, then cooled to 100-120°C and kept warm for 30 minutes, and then cooled to room temperature. A polyurethane adhesive layer is coated on one side of the softened PMMA / APET co-extruded laminated film, and then the side of the PET film coated with the silicone resin is composited on both sides of the main film to form an integral mobile phone screen protective film. The surface of the formed mobile phone screen protective film is sprayed with a reinforcing coating and an electrostatic film, and kept warm at a temperature of 110-120°C for 5-7 hours to obtain a pretreated tempered film. The pretreated tempered film is kept warm at a temperature of 150-160°C for 3-5 hours to obtain an optical film.

[0052] The above description of the disclosed embodiments is intended to enable one skilled in the art to implement or use the present invention. Various modifications to these embodiments will be readily apparent to one skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention is not limited to the embodiments shown herein but is intended to conform to the widest scope consistent with the principles and novel features disclosed herein.

Claims

1. A method for manufacturing a mobile phone optical film, characterized in that: It includes a hardening layer, a primer layer, a silicone layer and a substrate layer stacked in sequence from top to bottom, the substrate layer is an electrostatic film, the thickness of the substrate layer is 25-100μm, the thickness of the electrostatic film is 0.1mm to 0.8mm, the hardening layer, primer layer, silicone layer and substrate layer are made into a main film, PET films are arranged on both sides of the main film, the main film also includes a PMMA / APET co-extruded laminated film and a TPU film, a reinforcing film is coated on the surface of the main film, a water-based peelable glue is arranged on the surface of the substrate layer, an optical functional resin is arranged on the side of the substrate layer away from the water-based peelable glue, a heavy release film is arranged on the bottom surface of the silicone layer, an OCA anti-blue light material high viscosity layer is introduced on the silicone layer, a medium release film is arranged on the OCA anti-blue light material high viscosity layer, and a coating liquid with a color-changing effect is coated on the PET film and the OCA anti-blue light material high viscosity layer; The method for making the diaphragm also includes the following steps: Step 1: Slice the electrostatic film into uniform specifications; Step 2: hot-press the sliced ​​electrostatic film at a temperature of 80°C to 90°C, glue or apply glue to the die-cut electrostatic film, and set a transparent glue layer around the outer edge of the electrostatic film, wherein the peel strength of the glue layer is less than 20gf / inch, and the film is ready for use; Step 3: coating one side of the substrate layer with a water-based peelable glue and the other side with an optical functional resin; Step 4: Apply a coating liquid with a color-changing effect on the PET film by nano-coating; Step 5: Apply a layer of flexo color on the coated side, a layer of UV transfer texture on the coated side, and electroplate behind the texture; Step 6: Take the coated substrate layer, first coat the upper layer of the substrate layer with a primer liquid on one side, heat it in an oven to volatilize the solvent, and then perform UV curing to obtain a primer layer, thus completing the first coating step; Step 7: After the first coating step is completed, a high-ductility hardening coating liquid is coated on the upper layer of the primer layer, and then heated in an oven to volatilize the solvent, and then UV-cured to obtain a high-ductility hardening layer, completing the second coating step; Step 8, softening the PMMA / APET co-extruded laminated film, heating the PMMA / APET co-extruded laminated film to 200-210°C and keeping it warm for 30 minutes, then cooling it to 100-120°C and keeping it warm for 30 minutes, and then cooling it to room temperature; Step 9: coating one side of the softened PMMA / APET co-extruded laminated film with a polyurethane adhesive layer, and then laminating the side of the PET film coated with a silicone resin to both sides of the main film to form an integral mobile phone screen protective film; Step 10, spraying a reinforcing coating and an electrostatic film on the surface of the formed mobile phone screen protective film, keeping the temperature at 110-120° C. for 5-7 hours, and obtaining a pre-treated tempered film; Step 11: keep the pretreated tempered film at a temperature of 150-160° C. for 3-5 hours to obtain an optical film; The enhanced film is made by the following steps: Step 1: Add styrene, hydroxyethyl methacrylate, azobisisobutylnitrile and ethyl acetate into a reaction kettle, stir and mix, then add 3-butylenetriethoxysilane to react, cool and add triethylamine to neutralize to obtain a first intermediate, and react hydroxyethyl methacrylate, dodecafluoroheptyl methacrylate, isooctyl acrylate, styrene, azobisisobutylnitrile and tetrahydrofuran to obtain a second intermediate; Step 2: Add the first intermediate, the second intermediate, toluene-3,5-diisocyanate, and N,N-dimethylformamide into a reaction kettle, stir, add dibutyltin dilaurate, and react to obtain a third intermediate; add the third intermediate, methyltriethoxysilane, KH560, and xylene into a reaction kettle, stir, add deionized water, adjust the pH value of the reaction solution, and react together to obtain a fourth intermediate; Step 3: Add the fourth intermediate, antibacterial agent, potassium hydroxide and N,N-dimethylformamide into a reaction kettle to react and obtain a reinforcing liquid; mix the reinforcing liquid, nano titanium dioxide and defoaming agent evenly to obtain a reinforcing coating; apply the reinforcing coating to form a reinforcing film.

2. The method for manufacturing a mobile phone optical film according to claim 1, characterized in that: In the first coating step, the base coat is coated by a micro-concave coating method, the rotation speed of the coating roller is 3 to 17 m / min, the feed speed of the substrate is 5 to 25 m / min, the oven temperature is 60 to 150 °C, the curing time is 2 to 5 min, and the UV curing energy is 100 to 300 mJ / cm2. In the second coating step, the high ductility hardened layer (1) is coated by a micro-concave coating method, the rotation speed of the coating roller is 3 to 17 m / min, the feed speed of the substrate after coating the base coat (2) is 5 to 25 m / min, the oven temperature is 60 to 150 °C, the curing time is 2 to 4 min, and the UV curing energy is 100 to 600 mJ / cm2.

3. The method for manufacturing a mobile phone optical film according to claim 1, characterized in that: The water-based peelable glue comprises water-based polyurethane emulsion, water-based acrylic emulsion release agent and water, and is coated by slit extrusion coating, gravure coating or screen printing coating.

4. The method for manufacturing a mobile phone optical film according to claim 3, characterized in that: The weight percentage of the aqueous polyurethane emulsion is between 19.5% and 60%, the weight percentage of the aqueous acrylic emulsion release agent is between 0.5% and 20%, and the weight percentage of water is between 20% and 80%.

5. The method for manufacturing a mobile phone optical film according to claim 1, characterized in that: The hardened layer comprises, by weight percentage, 30% to 45% of a polymer with hexafunctional unsaturated functional groups, 45% to 63% of a solvent, 2% to 8% of an initiator, and 1% to 5% of an additive; the primer layer comprises, by weight percentage, 20% to 55% of a polymer with trifunctional or tetrafunctional unsaturated functional groups, 40% to 75% of a solvent, and 2% to 8% of an initiator.