A method for extracting aluminum hydroxide from fly ash at low temperature and normal pressure at one time

Through the method of one-time extraction of aluminum hydroxide at low temperature and normal pressure, using fly ash and other raw materials, it solves the problems of fly ash accumulation and high aluminum hydroxide production cost, realizes resource reuse and environmental protection, and reduces production costs.

CN116443904BActive Publication Date: 2024-10-25张珊珊
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310432998.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-04-20
Publication Date
2024-10-25
Estimated Expiration
2043-04-20

AI Technical Summary

Technical Problem

The long-term accumulation of fly ash occupies land resources, leading to soil and water environmental pollution. The existing aluminum hydroxide production method is costly, wastes resources, and relies on imported bauxite.

Method used

The method of one-time extraction of aluminum hydroxide at low temperature and normal pressure is adopted. Through the steps of batching, sintering and desiliconization, fly ash, quicklime, sodium carbonate and coal are used to optimize the batching ratio and sintering temperature to achieve low-cost production of aluminum hydroxide. .

Benefits of technology

It reduces the production cost of aluminum hydroxide, promotes resource reuse and environmental protection, reduces dependence on imported bauxite, and effectively solves the problem of high cost of fly ash reuse and recycling.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The embodiment of the present invention discloses a method for extracting aluminum hydroxide from fly ash at low temperature and normal pressure at one time, and the method comprises the following steps: batching, sintering, and desiliconization; wherein the raw materials of the batching are composed of fly ash, quicklime, sodium carbonate, and coal products in a mass ratio of 0.9-1.1: 0.9-1.1: 0.36-0.48: 0.13-0.18. The method provided by the present invention not only reduces the amount of quicklime used and reduces the cost of raw materials, but also realizes the conversion of sodium aluminate at a lower sintering temperature, greatly reducing the sintering cost, and the obtained sintered clinker can be desiliconized at normal temperature and pressure, reducing production costs. The present invention realizes the recycling of fly ash, protects the environment, turns waste into treasure, effectively solves the current situation that fly ash cannot be recycled or the recycling cost is high, and reduces the production cost of aluminum hydroxide.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The embodiment of the present invention relates to the technical field of development and utilization of fly ash, and specifically to a method for extracting aluminum hydroxide from fly ash at low temperature and normal pressure in one step. Background Art

[0002] Fly ash is the main solid waste produced after coal combustion, and its main components are oxides such as aluminum, silicon and iron. Thermal power plants discharge a large amount of fly ash every year. The long-term accumulation of fly ash has the following hazards: it occupies a large amount of land resources, and the harmful elements in the fly ash will penetrate into the soil and surrounding waters under the action of rainwater, thereby causing serious pollution to the soil and water environment; in windy weather, the fly ash dust will pollute a large area of ​​surrounding sites and air. Therefore, the reduction, harmlessness and resource utilization of fly ash are imminent.

[0003] The industrial production method of aluminum hydroxide mostly adopts the Bayer process. The main process of the Bayer process is: using alkali to react with aluminum oxide to generate soluble sodium aluminate, then stirring and decomposing the cooled sodium aluminate solution, filtering and separating to obtain the aluminum hydroxide product. The Bayer process requires the use of aluminum silicon ratio (Al 2 O 3 / SiO 2 )>7 high-grade aluminum ore. At the same time, before sintering, the raw materials need to be desiliconized under high temperature and high pressure conditions, which results in high production costs and great waste of resources.

[0004] Therefore, providing a method for extracting aluminum hydroxide using fly ash as raw material with low production cost is of great significance for resource recycling and ecological protection of the environment. Summary of the invention

[0005] To this end, an embodiment of the present invention provides a method for extracting aluminum hydroxide from fly ash at low temperature and normal pressure in one go. This method not only solves the problem of fly ash recycling, but also greatly reduces the production cost of aluminum hydroxide, greatly promotes resource recycling and environmental protection, effectively alleviates dependence on imported bauxite, and protects foreign exchange reserves.

[0006] In order to achieve the above objectives, the embodiments of the present invention provide the following technical solutions:

[0007] According to a first aspect of an embodiment of the present invention, there is provided a method for extracting aluminum hydroxide from fly ash at low temperature and normal pressure in one step, the method comprising the following steps: batching, sintering, and desiliconization; wherein the raw materials of the batching are composed of fly ash, quicklime, sodium carbonate and coal products in a mass ratio of 0.9-1.1:0.9-1.1:0.36-0.48:0.13-0.18.

[0008] The study found that in the batching process, adding coal products plays a role in combustion, making the sintering of the balls uniform and helping the chemical reaction of the raw materials. The applicant further optimized the amount of each material in the batching step and found that under the above mass ratio, while ensuring the aluminum recovery rate, it is more conducive to reducing the sintering temperature, achieving low-temperature sintering, and reducing the sintering cost.

[0009] In some preferred embodiments, the coal product is coal or coal gangue. The coal product is preferably coal gangue, which is conducive to further reducing production costs.

[0010] In some preferred embodiments, the mass ratio of the fly ash, quicklime, sodium carbonate and coal gangue is 1:1:0.44:0.15.

[0011] In some preferred embodiments, the sintering is carried out under normal pressure at a sintering temperature of 750-1030° C. If a rotary kiln is used for sintering, the sintering time is 20 min-2 h, and if a vertical kiln is used for sintering, the sintering time is 2-4 h.

[0012] In some preferred embodiments, the desiliconization specifically includes: cooling the sintered clinker, adding 70-100°C water, stirring, standing and settling, collecting the upper liquid phase, adding aluminum hydroxide seeds to the upper liquid phase for carbonization, filtering, dispersing the obtained solid phase in water, filtering again, and drying to obtain the aluminum hydroxide. The main components of the clinker are sodium aluminate and red mud, and the upper liquid phase is an aqueous solution mainly containing sodium aluminate.

[0013] In some preferred embodiments, before the sintering step, the method further comprises: adding water to the batched mixture and stirring to form balls.

[0014] In some preferred embodiments, the amount of water used is 2-10% of the mass of the mixture; the diameter of the ball is 4-10 cm. The size of the pellets has a significant impact on the recovery rate of aluminum. If the size of the pellets is too large, they cannot be burned through and the chemical combination is insufficient. If the size is too small, aluminum and red mud will form silicon slag together, resulting in a low dissolution rate. Research and development has found that within the above size range, the aluminum recovery rate can be significantly improved.

[0015] The embodiments of the present invention have the following advantages:

[0016] The method provided by the present invention not only reduces the amount of quicklime used and reduces the cost of raw materials, but also realizes the conversion of sodium aluminate at a relatively low sintering temperature, greatly reducing the sintering cost. The obtained sintered clinker can be desiliconized at normal temperature and pressure, reducing the production cost.

[0017] The invention realizes the renewable resource utilization of fly ash, protects the environment, turns waste into treasure, effectively solves the current situation that fly ash cannot be recycled or the recycling cost is high, and reduces the production cost of aluminum hydroxide. DETAILED DESCRIPTION

[0018] The following is a description of the implementation of the present invention by specific embodiments. People familiar with the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0019] If no specific techniques or conditions are specified in the examples, the techniques or conditions described in the literature in the field or the product instructions are used. If no manufacturer is specified for the reagents or instruments used, they are all conventional products that can be purchased through regular channels.

[0020] In the following embodiments: fly ash comes from power plant waste, and its aluminum oxide content is 35%-55%, and its silicon dioxide content is 45%-55%; coal gangue comes from Shanxi and Inner Mongolia.

[0021] Example 1

[0022] This embodiment provides a method for extracting aluminum hydroxide from fly ash at low temperature and normal pressure in one go:

[0023] Quicklime, sodium carbonate and coal gangue are ball-milled respectively to obtain powders with a particle size of about 200 mesh;

[0024] The fly ash is mixed with the ball-milled quicklime, sodium carbonate and coal gangue in a mass ratio of 1:1:0.44:0.15, and mixed evenly. 5% of water is added to the obtained mixture, and stirred to form pellets with a diameter of 4-10 cm to obtain raw meal;

[0025] The obtained raw material is fed into a rotary kiln and sintered at 780°C for 20 min to obtain clinker;

[0026] The obtained clinker is cooled to room temperature, stirred and precipitated by adding 70-80℃ water, and the supernatant sodium aluminate solution is separated. Aluminum hydroxide seeds are added to the supernatant for carbonization, and then the solid phase is collected by a filter press. The obtained solid phase is dispersed in water, and the sodium carbonate in the solid phase is removed. The solid phase is then put into the filter press again for drying. After the moisture content reaches the industrial standard, the obtained aluminum hydroxide can be bagged. After testing, the aluminum recovery rate is 93%.

[0027] Example 2

[0028] This embodiment provides a method for extracting aluminum hydroxide from fly ash at low temperature and normal pressure at one time:

[0029] Quicklime, sodium carbonate and coal gangue are ball-milled respectively to obtain powders with a particle size of about 200 mesh;

[0030] The fly ash is mixed with the ball-milled quicklime, sodium carbonate and coal gangue in a mass ratio of 0.9:1:0.38:0.18, and mixed evenly. 8% of water is added to the obtained mixture, and stirred to form a pellet with a diameter of 4-10 cm to obtain a raw meal;

[0031] The obtained raw material is fed into a rotary kiln and sintered at 850°C for 40 min to obtain clinker;

[0032] The obtained clinker is cooled to room temperature, stirred and precipitated by adding 70-80℃ water, and the supernatant sodium aluminate solution is separated. Aluminum hydroxide seeds are added to the supernatant for carbonization, and then the solid phase is collected by a filter press. The obtained solid phase is dispersed in water, and the sodium carbonate in the solid phase is removed. The solid phase is then put into the filter press again for drying. After the moisture content reaches the industrial standard, the obtained aluminum hydroxide can be bagged. After testing, the aluminum recovery rate is 89%.

[0033] Example 3

[0034] This embodiment provides a method for extracting aluminum hydroxide from fly ash at low temperature and normal pressure at one time:

[0035] Quicklime, sodium carbonate and coal gangue are ball-milled respectively to obtain powders with a particle size of about 200 mesh;

[0036] The fly ash is mixed with the ball-milled quicklime, sodium carbonate and coal gangue in a mass ratio of 1:1.1:0.42:0.13, and mixed evenly. 8% of water is added to the obtained mixture, and stirred to form pellets with a diameter of 4-10 cm to obtain raw meal;

[0037] The obtained raw material is fed into a rotary kiln and sintered at 780°C for 1 hour to obtain clinker;

[0038] The obtained clinker is cooled to room temperature, stirred and precipitated by adding 70-80℃ water, and the supernatant sodium aluminate solution is separated. Aluminum hydroxide seeds are added to the supernatant for carbonization, and then the solid phase is collected by a filter press. The obtained solid phase is dispersed in water, and the sodium carbonate in the solid phase is removed. The solid phase is then put into the filter press again for drying. After the moisture content reaches the industrial standard, the obtained aluminum hydroxide can be bagged. After testing, the aluminum recovery rate is 87%.

[0039] Example 4

[0040] This embodiment provides a method for extracting aluminum hydroxide from fly ash at low temperature and normal pressure at one time:

[0041] Quicklime, sodium carbonate and coal gangue are ball-milled respectively to obtain powders with a particle size of about 200 mesh;

[0042] The fly ash is mixed with the ball-milled quicklime, sodium carbonate and coal gangue in a mass ratio of 1:1:0.36:0.18, and mixed evenly. 10% of water is added to the obtained mixture, and stirred to form a pellet with a diameter of 4-10 cm to obtain a raw meal;

[0043] The obtained raw material is fed into a vertical kiln and sintered at 825°C for 2.5 hours to obtain clinker;

[0044] The obtained clinker is cooled to room temperature, stirred and precipitated by adding 70-100℃ water, and the supernatant sodium aluminate solution is separated. Aluminum hydroxide seeds are added to the supernatant for carbonization, and then the solid phase is collected by a filter press. The obtained solid phase is dispersed in water, and the sodium carbonate in the solid phase is removed. The solid phase is then put into the filter press again for drying. After the moisture content reaches the industrial standard, the obtained aluminum hydroxide can be bagged. After testing, the recovery rate of aluminum is 90%.

[0045] Example 5

[0046] This embodiment provides a method for extracting aluminum hydroxide from fly ash at low temperature and normal pressure in one go:

[0047] Quicklime, sodium carbonate and coal gangue are ball-milled respectively to obtain powders with a particle size of about 200 mesh;

[0048] The fly ash is mixed with the ball-milled quicklime, sodium carbonate and coal gangue in a mass ratio of 1:0.9:0.48:0.15, and mixed evenly. 6% of water is added to the obtained mixture, and stirred to form pellets with a diameter of 4-10 cm to obtain raw meal;

[0049] The obtained raw material is fed into a vertical kiln and sintered at 930°C for 2 hours to obtain clinker;

[0050] The obtained clinker is cooled to room temperature, stirred and precipitated by adding 75-85℃ water, and the supernatant sodium aluminate solution is separated. Aluminum hydroxide seeds are added to the supernatant for carbonization, and then the solid phase is collected by a filter press. The obtained solid phase is dispersed in water, and the sodium carbonate in the solid phase is removed. The solid phase is then put into the filter press again for drying. After the moisture content reaches the industrial standard, the obtained aluminum hydroxide can be bagged. After testing, the aluminum recovery rate is 88%.

[0051] Comparative Example 1

[0052] This comparative example provides a method for extracting aluminum hydroxide:

[0053] The quicklime is ball-milled to obtain a powder with a particle size of about 200 mesh;

[0054] The fly ash and the ball-milled quicklime are mixed in a mass ratio of 1:2, and 6% water is added to the obtained mixture, and the mixture is stirred to form a pellet with a diameter of 4-10 cm to obtain a raw meal;

[0055] The obtained raw material is fed into a rotary kiln and sintered at 750°C for 2h to obtain clinker;

[0056] The obtained clinker is cooled to room temperature, stirred and precipitated by adding 70-80℃ water, and the supernatant sodium aluminate solution is separated. Aluminum hydroxide seeds are added to the supernatant for carbonization, and then the solid phase is collected by a filter press. The obtained solid phase is dispersed in water, and the sodium carbonate in the solid phase is removed. The solid phase is then put into the filter press again for drying. After the moisture content reaches the industrial standard, the obtained aluminum hydroxide can be bagged. After testing, the aluminum recovery rate is 87%.

[0057] Although the present invention has been described in detail above by general description and specific embodiments, it is obvious to those skilled in the art that some modifications or improvements can be made to the present invention. Therefore, these modifications or improvements made without departing from the spirit of the present invention all belong to the scope of protection claimed by the present invention.

Claims

1. A method for extracting aluminum hydroxide from fly ash at low temperature and normal pressure at one time, characterized in that: The method comprises the following steps: batching, sintering, and desiliconization; wherein the raw materials of the batching are composed of fly ash, quicklime, sodium carbonate, and coal products in a mass ratio of 1:1:0.44:0.15; the coal products are coal gangue; the sintering is carried out at normal pressure and at 780°C for 20 minutes; the desiliconization specifically comprises: The sintered clinker is cooled, 70-100°C water is added, stirred, and allowed to stand for precipitation, the upper liquid phase is collected, aluminum hydroxide seeds are added to the upper liquid phase for carbonization, filtered, the obtained solid phase is dispersed in water, filtered again, and dried to obtain the aluminum hydroxide.

2. The method for extracting aluminum hydroxide from fly ash at low temperature and normal pressure at one time according to claim 1, characterized in that: Before the sintering step, the method further comprises: adding water to the batched mixture and stirring to form balls.

3. The method for extracting aluminum hydroxide from fly ash at low temperature and normal pressure at one time according to claim 2, characterized in that: The amount of water used is 2-10% of the mass of the mixture; and the diameter of the ball is 4-10 cm.

4. The method for extracting aluminum hydroxide from fly ash at low temperature and normal pressure at one time according to claim 1, characterized in that: The particle sizes of the quicklime, sodium carbonate and coal gangue are 180-220 meshes.