A low alloy high strength steel plate for pressure vessel and its manufacturing method
By introducing Al2O3+REM2O3 composite inclusions into low-alloy high-strength steel plates, solid solution N and Ti elements are absorbed to form Al2O3+TiN+REM2O3 composite inclusions, which solves the existing technology problems of increased steel plate thickness and high cost of using Ni elements. , achieving a combination of high strength and excellent welding performance to meet the safety and efficiency requirements of pressure vessels.
Patent Information
- Application Number
- CN202210016140.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-01-07
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2042-01-07
AI Technical Summary
In the existing technology, in order to improve the working pressure and welding performance of pressure vessels, it is usually necessary to increase the thickness of the steel plate and use expensive Ni elements, resulting in high production costs and insufficient strength, which cannot meet the use needs of pressure vessels.
Low-alloy high-strength steel plates are used, which contain a large number of fine Al2O3+REM2O3 composite inclusions. These composite inclusions pin austenite grains in the welding heat-affected zone and absorb solid solution N and Ti elements to form Al2O3+TiN +REM2O3 composite inclusions improve the welding performance against large linear energy.
It achieves high strength and excellent resistance to high-radial energy welding performance, improves manufacturing efficiency and low-temperature impact toughness of the welding heat-affected zone, and can reduce the wall thickness of pressure vessels while ensuring their safe and stable operation.
Smart Images

Figure BDA0003460896260000141 
Figure BDA0003460896260000142 
Figure BDA0003460896260000151
Abstract
Description
Technical Field
[0001] The invention relates to a metal material and a manufacturing method thereof, and in particular to a low-alloy high-strength steel plate and a manufacturing method thereof. Background Art
[0002] In recent years, with the increase in energy demand, in order to improve energy supply capacity and meet the growing domestic energy demand, energy production companies hope to increase the working pressure of pressure vessels for energy production to increase the rate of chemical reactions, thereby improving energy production efficiency.
[0003] In order to obtain more energy, companies often manufacture more reaction vessels and continuously increase the volume and pressure of pressure vessels to improve production efficiency. When the volume of the container becomes larger and the working pressure increases, designers generally need to consider increasing the thickness of the steel to ensure the safety of the pressure vessel. However, this design concept also brings many problems: on the one hand, the increase in the thickness of the steel plate will lead to low welding efficiency and affect the manufacturing efficiency of the pressure vessel; on the other hand, the large volume of the pressure vessel also brings various problems to the manufacturing, transportation and installation of the container.
[0004] In addition, according to the design and construction specifications of pressure vessels, if you want to increase the working pressure of the pressure vessel, you must increase the strength of the steel plate used to build the container, while ensuring its toughness, especially the toughness of the welded joints.
[0005] Based on this, in order to meet market demand, the present invention hopes to obtain a low-alloy high-strength steel plate for pressure vessels that can withstand high-energy line welding and has high strength. The steel plate has excellent resistance to high-energy line welding, and can be used for high-energy line welding when manufacturing pressure vessels, thereby improving welding efficiency and improving low-temperature impact toughness at the welding heat-affected zone. At the same time, this steel plate also has high strength, which can reduce the wall thickness of the pressure vessel while ensuring the safety of the pressure vessel operation.
[0006] Of course, in the prior art, some researchers have studied and designed some steel plates that are suitable for high-energy line welding:
[0007] For example, the Chinese patent document with publication number CN1962916A, publication date May 16, 2007, and titled "A Nb-Ti microalloyed steel suitable for high-energy-line welding and smelting method" discloses a Nb-Ti microalloyed steel suitable for high-energy-line welding, whose chemical composition is (weight %): C: 0.06% to 0.12%, Si: 0.10% to 0.50%, Mn: 0.40% to 1.8 %, P: ≤0.015%, S: ≤0.010%, Nb: 0.020%~0.050%, Ti: 0.006%~0.030%, N: 0.0030%~0.0100%, and may also contain one or more of Mo: ≤0.40%, V: ≤0.06%, Ni: ≤1.0%, Cr: ≤1.0%, Cu≤0.50%, and the balance is Fe and unavoidable inclusions. The steel plate produced by the invention can withstand high-energy-line welding of 50~150KJ / cm, but the high-energy-line welding level it can adapt to is relatively low, and cannot meet the welding energy-line requirements for the production of pressure vessels. .
[0008] Another example is the Chinese patent document with publication number CN103103451A, publication date May 15, 2013, and titled “High-energy-line welding low-temperature steel with yield ratio ≤ 0.85 and production method thereof”, which discloses a high-energy-line welding low-temperature steel with yield ratio ≤ 0.85, the components and weight percentage of which are: C: 0.04% to 0.07%, Si ≤ 0.20%, Mn: 0.8% to 1.2%, P: ≤ 0.0 13%, S: ≤0.003%, Ni: 0.35%~0.85%, Cr: 0.10%~0.30%, Ti: 0.008%~0.02%, Nb: 0.01%~0.02%, N: ≤0.005%; and meet: Nb≤0.358C, Ti / N is 2.5~3.5; The notable feature of this technical solution is also to improve the welding performance of the steel plate by adding a higher content of Ni element, and its production cost is relatively high.
[0009] Another example is the Chinese patent document with publication number CN1946862A, publication date April 11, 2007, and titled "Thick high-strength steel plate with excellent low-temperature toughness of heat-affected zone of welding by large heat input welding". The invention provides a thick high-strength steel plate, which can achieve excellent welding HAZ toughness when welding a steel plate with a thickness of 50-80 mm and a base material tensile strength of 490-570 MPa with a welding heat input of 20-100 kJ / mm. The thick high-strength steel plate contains C: 0.03-0.14%, Si: 0.30% Below, Mn: 0.8-2.0%, P: below 0.02%, S: below 0.005%, Ni: 0.8-4.0%, Nb: 0.003-0.040%, Al: 0.001-0.040%, N: 0.0010-0.0100%, Ti: 0.005-0.030%, Ni and Mn satisfy the formula: Ni / Mn≥10×Ceq-3(0.36<Ceq<0.42); wherein, Ceq=C+Mn / 6+(Cr+Mo+V) / 5+(Ni+Cu) / 15. When designing the chemical composition of the technical solution, the inventor added a large amount of Ni element to the steel to improve the low temperature toughness and high line energy welding resistance of the steel plate, resulting in a high production cost of such steel plates.
[0010] It can be seen from the above patent technical documents that in the prior art, current researchers mostly improve the steel plate's resistance to high-heat-line welding by adding the relatively expensive Ni element to the steel, and this design will lead to an increase in production costs. In addition, the steel plate tissue types involved in the above-listed technical solutions are mostly ferrite tissues, which determines that their strength is relatively low and cannot meet the use requirements of pressure vessels. Summary of the invention
[0011] One of the objects of the present invention is to provide a low-alloy high-strength steel plate for pressure vessels, wherein the low-alloy high-strength steel plate for pressure vessels has a large number of finely dispersed Al2O3+REM2O3 composite inclusions, wherein the composite inclusions can be used to pin the growth of austenite grains in the welding heat affected zone, and these composite inclusions can be used as nucleation cores to absorb the dissolved N and Ti elements in the heat affected zone, precipitate TiN precipitation phases, form Al2O3+TiN+REM2O3 composite inclusions, reduce the dissolved nitrogen content in the heat affected zone, and thereby greatly improve the steel plate's resistance to high line energy welding.
[0012] The low-alloy high-strength steel plate for pressure vessels described in the present invention has high strength and excellent resistance to large linear energy welding performance; the steel can be used to produce pressure equipment using large linear energy welding, thereby improving manufacturing efficiency and improving the low-temperature impact toughness of the welding heat affected zone; at the same time, because the steel plate also has high strength, it can reduce the wall thickness of the pressure vessel while ensuring the safe and stable operation of the pressure vessel.
[0013] In order to achieve the above object, the present invention provides a low alloy high strength steel plate for a pressure vessel, which contains Fe and inevitable impurities, and further contains the following chemical elements in the following mass percentages:
[0014] C: 0.06~0.19%, Si: 0.15~0.65%, Mn: 0.30~0.80%, Cr: 2.05~3.35%, Mo: 0.40~1.25%, Al(s): 0.005~0.019 %, Nb: 0.015~0.055%, Ti: 0.008~0.020%, REM: 0.0005~0.0020%, N: 0.0030~0.0060%, B: 0.0005~0.0025%.
[0015] Furthermore, in the low-alloy high-strength steel plate for pressure vessels of the present invention, the mass percentage of each chemical element is:
[0016] C: 0.06~0.19%, Si: 0.15~0.65%, Mn: 0.30~0.80%, Cr: 2.05~3.35%, Mo: 0.40~1.25%, Al(s): 0.005~0.019%, Nb: 0.015~0.055%, Ti: 0.008~0.020%, REM: 0.0005~0.0020%, N: 0.0030~0.0060%, B: 0.0005~0.0025%; the balance is Fe and unavoidable impurities.
[0017] In the low alloy high strength steel plate for pressure vessels of the present invention, the design principles of the chemical elements are as follows:
[0018] C: A certain amount of C element must be added to the low-alloy high-strength steel plate for pressure vessels described in the present invention. Adding an appropriate amount of C element to the steel is beneficial to the low-temperature toughness and welding performance of the steel. In order to ensure the beneficial effect of the C element, the C element content in the steel should not be too high, so the upper limit of the C element content is controlled to be 0.19%.
[0019] It should be noted that the C element is also a good solid solution and precipitation strengthening element. Adding an appropriate amount of C to the steel can ensure that the steel contains a certain amount of solid solution C elements, thereby improving the strength of the steel. In addition, the C in the steel can also precipitate in the steel in the form of various carbides with strong carbide elements such as Cr and Mo in the steel under certain heat treatment conditions, thereby playing a role in precipitation strengthening.
[0020] Correspondingly, the C content in the steel should not be too low. When the C content in the steel is too low, the Ac1, Ac3, Ar1, and Ar3 phase transition point temperatures of the steel are high, which is not conducive to the formulation and implementation of the subsequent rolling process, and thus it is easy to form mixed crystal structures with different grain sizes in the steel during rolling, and these mixed crystal structures are extremely unfavorable to the low-temperature toughness of the invention steel, and also have a negative impact on the structure of the steel after welding due to the tissue inheritance effect. Therefore, the lower limit of the C content in the steel is controlled to 0.06%. Based on this, considering the performance of the steel, in the low-alloy high-strength steel plate for pressure vessels described in the present invention, the mass percentage of the C element is controlled between 0.06 and 0.19%.
[0021] Mn: In the low-alloy high-strength steel plate for pressure vessels described in the present invention, the Mn element can be used as a deoxidizer. The deoxidation process is relatively mild, and the molten steel can be pre-deoxidized. The oxygen level of the molten steel can be stably controlled within an appropriate range, which is convenient for the subsequent addition of deoxidizers to form a suitable type of inclusions. In addition, the Mn element is also an austenite stabilizing element. Adding an appropriate amount of the Mn element to the steel can expand the temperature range of stable existence of austenite and reduce the Ac1, Ac3, Ar1, and Ar3 phase transformation point temperatures of the steel, thereby creating favorable conditions for controlling rolling. In addition, the Mn element also has certain solid solution strengthening effects and fine grain strengthening effects. In order to improve the strength of the steel plate, a certain amount of the Mn element needs to be added to the steel, so the Mn element content in the steel is controlled to be not less than 0.30%.
[0022] However, it should be noted that the Mn content in the steel should not be too high. When the Mn content is greater than 0.80%, the Mn element is prone to segregation during the solidification of the molten steel, especially in the center of the continuous casting billet, which is prone to form a Mn segregation band. This segregation band is very easy to be inherited to the subsequent rolled steel plate, resulting in poor low-temperature toughness at half the thickness of the steel plate. Based on this, in order to ensure the performance of the steel plate, the mass percentage of the Mn element in the low-alloy high-strength steel plate for pressure vessels described in the present invention is controlled between 0.30 and 0.80%.
[0023] Si: In the low-alloy high-strength steel plate for pressure vessels described in the present invention, Si element is similar to Mn element, and it is also a weak deoxidizer. A certain amount of Si and Mn elements can be added to the steel for joint pre-deoxidation to control the oxygen level in the molten steel to a certain range, and then Al element and REM element are used for deoxidation to form a certain number of target inclusions in the steel. However, it should be noted that the Si content in the steel should not be too high. When the Si content in the steel is too high, the low-temperature toughness of the steel will deteriorate. At the same time, the Si element in the steel after welding will promote the formation of a large amount of MA structure in the welding structure. These MA components with very high hardness will seriously damage the toughness of the welding heat affected zone. Therefore, the upper limit of the Si element added in the steel is controlled to be 0.65%. Based on this, in the low-alloy high-strength steel plate for pressure vessels described in the present invention, the mass percentage of the Si element is controlled between 0.15 and 0.65%.
[0024] Cr: In the low-alloy high-strength steel plate for pressure vessels described in the present invention, adding an appropriate amount of Cr element can improve the hardenability of the steel, which is beneficial to the quenching of thick steel plates and improves the strength and hardness of the steel; at the same time, after adding the Cr element, a dense chromium oxide protective film can be formed on the surface of the steel, which prevents the surface of the steel plate from oxidizing and corroding to a deeper layer under high temperature conditions, and can protect the steel plate. In addition, the Cr element can react with the C element in the steel at an appropriate temperature to generate fine carbides such as Cr7C3, thereby producing a precipitation strengthening effect and improving the strength of the steel plate. It should be noted that the Cr element content in the steel should not be too high. When the Cr content added to the steel is high, the toughness-brittle transition temperature of the steel will increase, and the impact toughness will decrease significantly. Based on this, in the low-alloy high-strength steel plate for pressure vessels described in the present invention, the mass percentage of the Cr element is controlled between 2.05 and 3.35%.
[0025] Mo: In the low-alloy high-strength steel plate for pressure vessels described in the present invention, adding an appropriate amount of Mo element can improve the high-temperature strength performance and creep resistance of the steel when working at high temperatures; at the same time, Mo element can also improve the hardenability of thick steel plates, further improving the strength performance of the steel plates. However, after Mo element is added to steel, it will increase the Ac3, Ac1, Ar3, Ar1 phase transition point temperatures of the steel plate, which is also not conducive to the controlled rolling of the steel plate, and Mo element is expensive. After adding too much Mo element, the production cost of steel will be greatly increased. Based on this, considering the beneficial effects and adverse effects of Mo element, in the low-alloy high-strength steel plate for pressure vessels described in the present invention, the mass percentage of Mo element is controlled between 0.40 and 1.25%.
[0026] Al(s): In the low-alloy high-strength steel plate for pressure vessels described in the present invention, aluminum element serves as a strong deoxidizer, which can further control the oxygen position of molten steel before the final deoxidation of REM elements, thereby preparing for the final deoxidation of REM elements. It should be noted that when the Al(s) content in the steel is low, the oxygen position of the molten steel cannot meet the final deoxidation requirements of REM elements; and when the Al(s) content in the steel is high, magnesium-aluminum spinel inclusions are easily formed in the steel, which damages the mechanical properties of the steel plate, and is also not conducive to controlling the formation of Al2O3+TiN+REM2O3 composite inclusions in the steel after welding. Therefore, considering the influence of the Al(s) content on the performance of the steel plate, in the low-alloy high-strength steel plate for pressure vessels described in the present invention, the mass percentage of Al(s) is controlled between 0.005 and 0.019%.
[0027] In addition, it should be noted that Al(s) in steel can react with part of the N element in the heat affected zone after welding, reduce the N element concentration at the HAZ position, and improve the toughness of the welding heat affected zone of the steel plate; at the same time, after Al(s) combines with N, it can prevent the B element in the steel from combining with N. After forming BN, the B element content in the steel is reduced, thereby weakening the hardenability of the B element in the steel. However, since the binding force between B and N is greater than the force between Al(s) and N, the Al(s) content needs to be increased accordingly. Therefore, in some preferred embodiments, in order to obtain a better implementation effect, while controlling the mass percentage of a single chemical element, the mass percentage of Al(s), N, and Ti can be further controlled to satisfy the following formula: 24×Al(s)≥10×(24×N-7×Ti).
[0028] Nb: In the low-alloy high-strength steel plate for pressure vessels described in the present invention, adding an appropriate amount of Nb element can effectively refine the microstructure of the steel and improve the strength and toughness of the steel; in addition, the Nb element can also combine with the C element in the steel to generate NbC precipitation phase, achieving the effect of grain refinement. However, it should be noted that the Nb element content in the steel should not be too high. When the Nb element content in the steel is too high, the toughness of the heat affected zone of the steel plate welding will be reduced. Based on this, in the low-alloy high-strength steel plate for pressure vessels described in the present invention, the mass percentage of the Nb element is controlled between 0.015 and 0.055%.
[0029] Ti: In the low-alloy high-strength steel plate for pressure vessels described in the present invention, the Ti element can be used as a deoxidizer. The deoxidation ability of the Ti element is slightly stronger than that of the Si element and the Mn element. Adding an appropriate amount of the Ti element to the steel can properly deep deoxidize to better control the oxygen position in the molten steel, which can generate suitable inclusion types in the steel when the Al element and the REM element are subsequently deoxidized. In addition, in addition to steelmaking deoxidation, there is also a part of the solid-dissolved Ti element in the steel. This part of the Ti element can be combined with part of the N element in the steel during the subsequent heat treatment process to form a TiN precipitation phase with good stability; these TiN precipitation phases can hinder the growth of austenite grains during the solidification process, refine the organization, and help improve the strength of the steel plate. In addition, after the steel plate is welded with a large line energy, when the solid-dissolved Ti and N content in the steel are appropriate, fine TiN can be formed. These fine TiN precipitation phases can refine the organization of the welding heat-affected zone, affect the secondary phase transformation products, and improve the low-temperature toughness of the welding heat-affected zone of the steel plate.
[0030] It should be noted that when the Ti content in the steel is high, the size of the TiN precipitate phase formed will become larger. Such coarse TiN particles cannot play the role of pinning the growth of austenite grains in the heat-affected zone, but may become the starting point of crack initiation, deteriorating the low-temperature impact toughness of the heat-affected zone after steel welding. Therefore, in order to give full play to the beneficial effect of the Ti element, in the low-alloy high-strength steel plate for pressure vessels described in the present invention, the mass percentage of the Ti element in the steel is controlled between 0.008 and 0.020%.
[0031] To this end, in some preferred embodiments, in order to give full play to the role of TiN precipitate phase particles in steel in pinning the growth of austenite grains during the thermal process of steel, while controlling the mass percentage of a single chemical element, the mass percentage of Ti and N elements in the steel can be controlled to satisfy Ti / N: 2.40 to 3.50.
[0032] REM: In the low-alloy high-strength steel plate for pressure vessels described in the present invention, adding an appropriate amount of REM elements to the steel is beneficial to controlling the oxygen level in the molten steel. Since the deoxidation capacity of REM is greater than that of the Al element, REM can react with the Al2O3 already generated in the molten steel to form an Al2O3+REM2O3 composite oxide; this Al2O3+REM2O3 composite oxide can pin the growth of austenite grains in the heat-affected zone of the welding during the subsequent welding process of the steel plate, thereby refining the austenite grain size and improving the high-energy line welding performance of the steel. In addition, during the cooling process, TiN can also be solid-state precipitated with the Al2O3+REM2O3 composite oxide as the core to obtain Al2O3+TiN+REM2O3 composite inclusions, further reducing the free N content near the welding heat-affected zone and better improving the low-temperature toughness of the heat-affected zone.
[0033] When the amount of REM added is large, a large amount of REM2O3 oxides will be formed in the molten steel. The size of the oxides is very easy to grow. Once large-sized REM2O3 oxides are formed, such oxides will not only fail to hinder the growth of austenite grains near the welding affected zone, but may become the source of crack initiation, producing harmful effects. Therefore, the upper limit of the amount of REM added in the steel is controlled to be 0.0020%; when the amount of REM added is small, the density of the Al2O3+REM2O3 composite oxides formed in the molten steel is too small, and the effect of these composite oxides in pinning the austenite grain size in the welding heat affected zone will also be greatly reduced. Therefore, the lower limit of the amount of REM added in the molten steel should be controlled to be 0.0005%. Based on this, in order to give full play to the beneficial effects of REM, in the low-alloy high-strength steel plate for pressure vessels described in the present invention, the mass percentage of REM is controlled between 0.0005 and 0.0020%.
[0034] Accordingly, in order to better form Al2O3+REM2O3 composite oxide, in some preferred embodiments, while controlling the mass percentage of a single chemical element, the mass percentage of Al(s) and REM in the steel can be further controlled to satisfy: 1 / 10≤REM / Al(s)≤1 / 5.
[0035] N: In the low-alloy high-strength steel plate for pressure vessels described in the present invention, the N element can combine with the partially dissolved Ti element in the steel to form a TiN precipitate phase with good stability. When the N content in the steel is less than 0.0030%, the TiN precipitate phase formed in the steel is relatively small, and it is difficult to satisfy the function of pinning austenite; and when the nitrogen content in the steel is too high, it will have an adverse effect on the toughness of the steel, especially when the dissolved nitrogen content exceeds 0.0060%, it will reduce the low-temperature toughness of the thick steel plate, and it is easy to form a coarse TiN precipitate phase in the heat-affected zone after welding, weakening the hindering effect of TiN on the growth of austenite grains near the HAZ. Based on this, in the low-alloy high-strength steel plate for pressure vessels described in the present invention, the mass percentage of the N element is controlled between 0.0030 and 0.0060%.
[0036] B: In the low-alloy high-strength steel plate for pressure vessels described in the present invention, the B element has a strong hardening effect in the steel. A small amount of B segregates at the austenite grain boundary, which can inhibit the formation of proeutectoid ferrite on the grain boundary and promote the formation of bainite, thereby improving the strength and toughness of the steel plate. In addition, the B element can also play an important role in the heat affected zone of welding, improving the low-temperature impact toughness of the organization near the fusion line of the welded joint. The main reasons are: on the one hand, B can combine with N to form BN, reduce the solid solution N content in the steel, and improve the low-temperature toughness of the steel; on the other hand, due to the unique crystallographic characteristics of BN, BN and ferrite directly have a low-energy orientation relationship, so the BN precipitation phase can induce the formation of a large number of needle-shaped ferrite organizations, further divide the original austenite grains, and effectively reduce the austenite grain size, thereby improving the low-temperature toughness near the fusion line.
[0037] However, it should be noted that the B element content in the steel should not be too high. When the B element content in the steel is too high, the solid-solution B element is easy to form a large amount of segregation at the grain boundary, which is not conducive to the performance of the steel after welding. Therefore, the upper limit of the B element content in the steel is controlled to be 0.0025%. Based on this, in the low-alloy high-strength steel plate for pressure vessels described in the present invention, the mass percentage of the B element is controlled between 0.0005 and 0.0025%.
[0038] At the same time, in order to fully exert the functions of TiN and BN, in some preferred embodiments, while controlling the mass percentage of a single chemical element, the mass percentage of Ti, B and N elements can be further considered to satisfy: [6+0.7714×(N-0.2916×Ti)]×10 -4 ≤B≤[25+0.7714×(N-0.2916×Ti)]×10 -4 .
[0039] When the Ti, B and N elements satisfy the above relationship, on the one hand, a certain amount of B can be contained in the steel plate before welding, which can promote the hardenability of the steel plate; on the other hand, after the steel plate is welded, the influence of TiN and BN on the phase transformation in the welding heat affected zone and the fusion line position of the weld joint can be fully exerted, thereby improving the welding performance of the steel plate.
[0040] Furthermore, the low alloy high strength steel plate for pressure vessels according to the present invention further contains at least one of the following chemical elements:
[0041] 0<Cu≤0.30%;
[0042] 0<Ni≤0.30%.
[0043] In the above technical solution of the present invention, both Cu and Ni elements can further improve the quality and performance of the low alloy high strength steel plate for pressure vessels of the present invention. Among them, Cu can improve the corrosion resistance of steel and increase the strength of steel, but when the Cu content in the steel is too high, high temperature brittleness is easily generated at high temperatures. Therefore, in the low alloy high strength steel plate for pressure vessels of the present invention, the mass percentage of the Cu element can be controlled to 0<Cu≤0.30%.
[0044] Correspondingly, adding a certain amount of Ni element to the steel can improve the low-temperature toughness and strength of the steel plate, but considering the high price of Ni element, in order to control the production cost, in the low-alloy high-strength steel plate for pressure vessels described in the present invention, the mass percentage of Ni element can be controlled to 0<Ni≤0.30%.
[0045] The addition of the above elements will increase the cost of the material. Taking into account the performance and cost control, in the technical solution described in the present invention, at least one of the above elements can be preferably added.
[0046] Furthermore, in the low alloy high strength steel plate for pressure vessels of the present invention, among other inevitable impurities: P≤0.010%, S≤0.010%.
[0047] In the above technical solution of the present invention, both P and S are impurity elements in the low-alloy high-strength steel plate for pressure vessels described in the present invention. When technical conditions permit, in order to obtain steel with better performance and higher quality, the content of impurity elements in the steel should be reduced as much as possible.
[0048] P: In the low-alloy high-strength steel plate for pressure vessels described in the present invention, the P element is a harmful impurity element. When the steel plate works at high temperature, the P element in the steel tends to segregate to the austenite grain boundary, causing the P element concentration at the austenite grain boundary to increase significantly, reducing the bonding force of the austenite grain boundary, and easily forming temper brittleness, which may eventually cause the steel plate to crack. Therefore, in the low-alloy high-strength steel plate for pressure vessels described in the present invention, it is hoped that the P content is as low as possible. In combination with steelmaking cost and operability, the mass percentage of the P element can be controlled to P≤0.010%.
[0049] S: In the low-alloy high-strength steel plate for pressure vessels described in the present invention, the impurity element S is very easy to combine with the Mn element in the steel during the solidification process of the steel to form MnS inclusions. Since the MnS inclusions have good high-temperature plasticity, MnS is easy to form long strips and large-sized inclusions extending along the rolling direction during the rolling process of the steel plate, thereby deteriorating the transverse performance, Z-direction performance and welding performance of the steel plate. Therefore, combined with the conditions of steelmaking cost and operability, in the low-alloy high-strength steel plate for pressure vessels described in the present invention, the mass percentage of the S element is controlled to S≤0.010%.
[0050] Furthermore, in the low-alloy high-strength steel plate for pressure vessels of the present invention, the mass percentage of each chemical element satisfies at least one of the following items:
[0051] Ti / N: 2.40~3.50;
[0052] 24×Al(s)≥10×(24×N-7×Ti);
[0053] [6+0.7714×(N-0.2916×Ti)]×10 -4 ≤B≤[25+0.7714×(N-0.2916×Ti)]×10 -4 ;
[0054] 1 / 10≤REM / Al(s)≤1 / 5;
[0055] In the above formula, each element is substituted with the mass percentage of the corresponding chemical element.
[0056] Furthermore, in the low alloy high strength steel plate for pressure vessels described in the present invention, it has Al2O3+REM2O3 composite inclusions.
[0057] Furthermore, after the low-alloy high-strength steel plate for the pressure vessel is welded with a high line energy of at least 200 KJ / cm, there are fine and dispersed Al2O3+REM2O3+TiN composite inclusions in the welding heat affected zone.
[0058] Furthermore, in the low-alloy high-strength steel plate for pressure vessels described in the present invention, the proportion of Al2O3+REM2O3 composite inclusions in all inclusions is greater than 40%.
[0059] In the above technical scheme of the present invention, the low-alloy high-strength steel plate for pressure vessels described in the present invention has a large number of finely dispersed spherical or nearly spherical Al2O3+REM2O3 composite inclusions. These composite inclusions can be used to pin the growth of austenite grains in the welding heat affected zone, and these composite inclusions can be used as nucleation cores to absorb the dissolved N and Ti elements in the heat affected zone, precipitate TiN precipitation phases, form Al2O3+TiN+REM2O3 composite inclusions, reduce the dissolved nitrogen content in the heat affected zone, and thus greatly improve the steel plate's resistance to high line energy welding.
[0060] Furthermore, in the low-alloy high-strength steel plate for pressure vessels described in the present invention, the average size of all inclusions is less than 5 μm, and the proportion of inclusions with a size of 5 to 8 μm to all inclusions is less than 1 / 1000, and the proportion of inclusions with a size greater than 8 μm to all inclusions is less than 1 / 10000.
[0061] Furthermore, in the low-alloy high-strength steel plate for pressure vessels described in the present invention, its yield strength is ≥450MPa, its tensile strength is ≥570MPa, and its low-temperature impact toughness at least at -30°C is ≥270J; after welding with a high line energy of at least 200KJ / cm, the low-temperature impact toughness of the welding heat-affected zone at at least -30°C is ≥135J.
[0062] Correspondingly, another object of the present invention is to provide a method for manufacturing a low-alloy high-strength steel plate for a pressure vessel, which adopts an optimized manufacturing process. By controlling the type, addition order, oxygen position and addition amount of the deoxidizer during the smelting process, a low-alloy high-strength steel plate for a pressure vessel with a large amount of Al2O3+REM2O3 composite inclusions can be obtained.
[0063] The low-alloy high-strength steel plate for pressure vessels obtained by the manufacturing method has high strength and excellent resistance to large linear energy welding performance, and can be used to manufacture pressure equipment, and has very good promotion prospects and application value.
[0064] In order to achieve the above object, the present invention proposes a method for manufacturing the above-mentioned low-alloy high-strength steel plate for pressure vessels, which comprises the steps of:
[0065] (1) Smelting and continuous casting: Deoxidizers Si, Mn, Ti, Al and REM are added during the smelting process of the molten steel; before the molten steel is cast, pre-deoxidation is carried out in the order of Si, Mn, Ti and Al, and the oxygen level of the cast molten steel is controlled to be 0.0045-0.0085%; then, REM is used for final deoxidation, and the mass percentage of REM in the molten steel is controlled to be 0.0005-0.0020%;
[0066] (2) Heating and rolling;
[0067] (3) Quenching + tempering.
[0068] In the present invention, in order to give full play to the pinning effect of Al2O3+TiN+REM2O3 composite oxides on austenite grains in the welding heat affected zone, it is necessary to form a large number of fine, uniform and dispersed Al2O3+REM2O3 composite inclusions in the invention steel. The prerequisite is that the change of oxygen level in molten steel during deoxidation must be accurately controlled. In order to control the oxygen level in molten steel, it is necessary to select appropriate deoxidizing elements and carry out deoxidation in a certain order of addition.
[0069] In step (1) of the manufacturing method of the present invention, the present invention adopts the order of adding Si, Mn, Ti, Al, and REM for deoxidation during the smelting process. First, Si+Mn is used for preliminary deoxidation, which can fix the oxygen position within a range suitable for subsequent deoxidation; then a proper amount of Ti is added for deoxidation to further reduce the free oxygen concentration in the molten steel. Since the interface energy of Ti2O3 inclusions is relatively small, it is not easy to aggregate and grow, and a large number of fine, spherical or nearly spherical dispersed Ti2O3 inclusions can be formed.
[0070] Then, in step (1), the oxygen level of the cast steel is controlled to be 0.0045-0.0085%, and an appropriate amount of Al element is added at an appropriate oxygen level for further deoxidation; since the deoxidation ability of Al element is stronger than that of Ti element, Ti in the Ti2O3 inclusions will be reduced, and Al atoms will replace the positions of Ti atoms, thereby forming a large number of dispersed, fine, uniformly distributed, spherical or nearly spherical Al2O3 inclusions.
[0071] Finally, REM is used for final deoxidation. After REM final deoxidation, part of the Al2O3 oxide inclusions are replaced by REM, thereby forming a large number of fine, dispersed, and evenly distributed Al2O3+REM2O3 composite oxides. These composite oxides will prevent the growth of austenite grain size during subsequent high-energy line welding of steel plates, thereby improving the low-temperature toughness and impact resistance of the steel plate near the weld.
[0072] When the low alloy high strength steel plate for pressure vessels described in the present invention is used, during the welding process, the Al2O3+REM2O3 composite inclusions in the steel can pin the growth of austenite grains in the welding heat affected zone, and can use these Al2O3+REM2O3 composite inclusions as nucleation cores to absorb TiN precipitation phases precipitated from the solid solution N element and Ti element in the heat affected zone, reduce the solid solution nitrogen content in the heat affected zone, and thus greatly improve the steel plate's resistance to high line energy welding.
[0073] Furthermore, in the manufacturing method of the present invention, in step (1), a light reduction process is adopted at the end of solidification of the continuous casting billet, and the reduction rate is 5 to 12%.
[0074] Furthermore, in the manufacturing method of the present invention, in step (2), the ingot is heated to 1050-1180°C for rolling, the final rolling temperature is controlled to be greater than 900°C, and the total cumulative reduction ratio is greater than 65%.
[0075] In the above technical solution of the present invention, during the rolling process of step (2), the ingot needs to be firstly input into a heating furnace for heating, and preferably the ingot is heated to 1050-1180°C. This is because: when the heating temperature of the ingot is less than 1050°C, the carbides and nitrides of Nb in the ingot cannot be completely dissolved, which will reduce the pinning effect of Nb on austenite grains during the rolling process; and when the temperature of heating the ingot is higher than 1180°C, it is easy to cause the austenite grains to grow rapidly, affecting the performance of the steel.
[0076] Furthermore, in the manufacturing method described in the present invention, in step (2), two-stage controlled rolling is adopted: in the first stage, continuous single-pass large reduction rate rolling is adopted at above 970°C, the single-pass rolling reduction rate is not less than 16%, and the total reduction rate is not less than 69%; then in the second stage, the second stage rolling is carried out below 940°C, the single-pass rolling reduction rate is controlled to be not less than 9%, and the total reduction rate is not less than 38%.
[0077] Accordingly, in the present invention, when rolling steel, the final rolling temperature can be controlled to be greater than 900°C, the total cumulative reduction rate can be greater than 65%, and the above-mentioned two-stage rolling process can be used to control the rolling process. This is because: under the above-mentioned thermal deformation conditions, the steel can undergo complete recrystallization, thereby continuously refining the austenite; if the above-mentioned conditions are not met, larger austenite grains may exist in the steel, which will damage the strength and low-temperature toughness of the steel. Of course, in some embodiments, it is also preferred to control the final rolling temperature to be greater than 920°C.
[0078] Furthermore, in the manufacturing method described in the present invention, in step (3), the quenching temperature is controlled to be 860-960°C, the holding time is (1.2-2.9)×T min, and after the holding period is completed, the steel plate is taken out of the furnace and water-cooled to room temperature, wherein T represents the thickness of the steel plate in mm.
[0079] In the above technical solution of the present invention, in the quenching + tempering heat treatment process of step (3), the quenching temperature can be further controlled to be 860-960°C. This is because: when the quenching temperature is lower than 860°C, the homogenization of the austenite of the steel takes a long time and the efficiency is low; and when the quenching temperature of the steel is higher than 960°C, part of the austenite in the steel tends to grow and is prone to form a mixed crystal structure, which is not conducive to the uniformity of the steel structure.
[0080] In addition, during the quenching process, the holding time can be preferably controlled to be (1.2~2.9)×T min. This is because: when the holding time of the steel at the quenching temperature is less than 1.2T min, the steel cannot be fully austenitized; and when the holding time of the steel exceeds 2.9T min, it exceeds the time required for the steel to be austenitized, which will reduce the efficiency of the quenching process.
[0081] Furthermore, in the manufacturing method of the present invention, in step (3), the tempering temperature is controlled to be 690-755°C, and the holding time is (2.2-3.8)×T min, wherein T represents the thickness of the steel plate in mm.
[0082] In the present invention, when the tempering temperature of the steel is lower than 690°C, a longer tempering time is required to remove the residual quenching stress in the steel, which will reduce the tempering efficiency; when the tempering temperature of the steel is higher than 755°C, the dislocation density in the steel will drop significantly, thereby reducing the strength of the steel. During the tempering process, when the tempering holding time is lower than 2.2T min, the quenching stress of the steel cannot be completely removed; when the tempering holding time is higher than 3.8T min, the production efficiency of the tempering process will be reduced.
[0083] Compared with the prior art, the low alloy high strength steel plate for pressure vessels and the manufacturing method thereof according to the present invention have the following advantages and beneficial effects:
[0084] The low-alloy high-strength steel plate for pressure vessels described in the present invention adopts a reasonable chemical element composition design and is combined with an optimized manufacturing process. By properly controlling the deoxidizers, deoxidation sequence, oxygen level of molten steel and the amount of different deoxidizers used in the steel smelting process, a large number of fine, dispersed, evenly distributed spherical or nearly spherical Al2O3+REM2O3 composite oxides can be formed in the steel plate of the present invention.
[0085] These special composite inclusions can play the role of pinning the growth of austenite grains near the heat affected zone of welding when the steel of the present invention is subjected to high input energy welding. At the same time, during the cooling process after welding, a part of the dissolved N elements and dissolved Ti elements will precipitate with these special composite oxides as the core to form Al2O3+REM2O3+TiN composite oxides, thereby reducing the content of dissolved N elements near the heat affected position of welding, thereby increasing the low-temperature impact toughness of the heat affected zone of the steel plate, and ultimately improving the high input energy welding resistance of the invented steel plate.
[0086] The low-alloy high-strength steel plate for pressure vessels described in the present invention has high strength and excellent resistance to large linear energy welding. The steel can be used to produce pressure equipment by large linear energy welding, thereby improving manufacturing efficiency and increasing the low-temperature impact toughness of the welding heat-affected zone. At the same time, because the steel plate also has high strength, it can reduce the wall thickness of the pressure vessel while ensuring the stable and safe operation of the pressure vessel. DETAILED DESCRIPTION
[0087] The low-alloy high-strength steel plate for pressure vessels and the method for manufacturing the same according to the present invention will be further explained and illustrated below in conjunction with specific embodiments. However, such explanation and illustration do not constitute an improper limitation on the technical solution of the present invention.
[0088] Examples 1-7 and Comparative Examples 1-3
[0089] Table 1-1 and Table 1-2 list the mass percentages of the chemical elements of the low alloy high strength steel plates for pressure vessels of Examples 1-7 and the comparative steels of Comparative Examples 1-3 and the relationships between the chemical elements.
[0090] Table 1-1. (wt%, the balance is Fe and other inevitable impurities except P and S)
[0091]
[0092] Table 1-2
[0093]
[0094] The low alloy high strength steel plates for pressure vessels of Examples 1 to 7 of the present invention are all prepared by the following steps:
[0095] (1) Smelting and casting according to the chemical composition shown in Table 1-1 and Table 1-2: according to the alloy composition ratio of the invention steel, add appropriate amounts of Cr, Mo, Cu, Ni, and Nb alloys with the furnace; smelting is carried out under a vacuum of about 16 Pa at the lowest, and argon is filled for protection. After the pure iron is completely melted, add appropriate amounts of deoxidizers in the order of Si, Mn, Ti, Al, and REM. Among them, pre-deoxidation is carried out in the order of Si, Mn, Ti, and Al before molten steel is cast, and the oxygen level of the cast molten steel is controlled to be 0.0045-0.0085%; then REM is used for final deoxidation, and the mass percentage of REM in the molten steel is controlled to be 0.0005-0.0020%; then it is cast into a continuous casting billet, and a light reduction process is used at the end of solidification of the continuous casting billet, and the reduction rate is controlled to be 5-12%.
[0096] (2) Heating and rolling: The ingot is input into a heating furnace and heated to 1050-1180°C for rolling, and a two-stage controlled rolling is adopted. In the first stage, continuous single-pass large reduction rate rolling is adopted at above 970°C, the single-pass rolling reduction rate is not less than 16%, and the total reduction rate is not less than 69%; then in the second stage, the second stage rolling is carried out at below 940°C, the single-pass rolling reduction rate is controlled to be not less than 9%, and the total reduction rate is not less than 38%; during the rolling process, the final rolling temperature is controlled to be greater than 900°C, preferably greater than 920°C, and the total cumulative reduction rate is controlled to be greater than 65%, and the thickness of the rolled steel plate is 38 mm.
[0097] (3) Quenching + tempering: The quenching temperature is controlled at 860-960°C and the holding time is (1.2-2.9) × Tmin. After the holding period, the steel plate is taken out of the furnace and water-cooled to room temperature, where T represents the thickness of the steel plate in mm. The tempering temperature is controlled at 690-755°C and the holding time is (2.2-3.8) × Tmin, where T represents the thickness of the steel plate in mm.
[0098] It should be noted that, in the present invention, the chemical composition design and related processes of the low-alloy high-strength steel plates for pressure vessels in Examples 1-7 all meet the design specification requirements of the present invention.
[0099] Correspondingly, although the comparative steels of Comparative Examples 1-3 are also produced by the above process flow of "smelting, casting, heating, rolling, quenching and tempering", the deoxidation order of REM and Al is exchanged, and the other process conditions are within the scope of the present invention.
[0100] Table 2-1 and Table 2-2 list the specific process parameters of the low alloy high strength steel plates for pressure vessels of Examples 1-7 and the comparative steels of Comparative Examples 1-3 in the above process steps.
[0101] Table 2-1.
[0102]
[0103]
[0104] Table 2-2.
[0105]
[0106] In the above Table 2-1 of the present invention, since the first-stage rolling and the second-stage rolling are specifically subdivided into several passes, rather than just one value, the single-pass reduction ratios of the first and second stages of each embodiment and comparative example in Table 2-1 are range values, rather than single point values.
[0107] It should be noted that when Examples 1-7 and Comparative Examples 1-3 are subjected to the above-mentioned manufacturing process, in step (1), after Examples 1-7 are pre-deoxidized in the order of Si, Mn, Ti and Al, and after Comparative Examples 1-3 are pre-deoxidized in the order of Si, Mn, Ti and REM, the molten steel obtained in each Example and Comparative Example can be sampled, and the oxygen level of the sample molten steel in each Example and Comparative Example can be tested, and the relevant test results are listed in the following Table 3.
[0108] Correspondingly, after the pre-deoxidation is completed, Example 1-7 will add REM for final deoxidation and control the mass percentage of REM in the molten steel; Comparative Example 1-3 will add Al for final deoxidation. The mass percentage of REM in the molten steel obtained in the final Example 1-7 and Comparative Example 1-3 is tested, and the results are also listed in the following Table 3.
[0109] Table 3.
[0110]
[0111]
[0112] The low-alloy high-strength steel plates for pressure vessels of the finished products of Examples 1-7 and the comparative steels of Comparative Examples 1-3 finally obtained through the above process steps were sampled respectively, and the inclusions of the sample steels of each Example and Comparative Example were observed and analyzed.
[0113] In the present invention, the inclusions in the steel can be extracted by electrolytic extraction, and the precipitated phases in different scale ranges can be separated by filter membranes with different pore sizes; the types and contents of the inclusions in the steel can be analyzed by SEM (scanning electron microscope) and EDS (Energy Dispersive Spectrometer) technology to confirm the chemical composition of the inclusions, the particle size distribution of the inclusions can be detected by a laser particle size analyzer, and the image analysis software can be used to finally confirm the number, volume density, type, aspect ratio and average size of the precipitated phases (inclusions) in the steel.
[0114] Through the above experiments, the average size of all inclusions in the sample steel materials of Examples 1-7 and Comparative Examples 1-3, the proportion of inclusions with a size of 5 to 8 μm in all inclusions, the proportion of inclusions with a size greater than 8 μm in all inclusions, and the proportion of Al2O3+REM2O3 composite inclusions in all inclusions can be determined. The inclusion observation and analysis results of the sample steel materials of Examples 1-7 and Comparative Examples 1-3 are listed in the following Table 4.
[0115] Table 4 lists the inclusion observation and analysis results of the low alloy high strength steel plates for pressure vessels of Examples 1-7 and the comparative steels of Comparative Examples 1-3.
[0116] Table 4.
[0117]
[0118]
[0119] As shown in Table 4, it was observed that the steel samples of Examples 1-7 and Comparative Examples 1-3 all had small, dispersed spherical Al2O3+REM2O3 composite inclusions. The inclusions in Comparative Examples 1-3 and Examples 1-7 were different due to the different order of adding deoxidizers during the deoxidation process.
[0120] From the comparison results, it can be seen that both Examples 1-7 and Comparative Examples 1-3 contain Al2O3+REM2O3 composite inclusions, but the proportion of Al2O3+REM2O3 composite inclusions in Example 1-7 to all inclusions is significantly higher than that in Comparative Examples 1-3, and the average diameter (average particle size) of all inclusions in Example 1-7 is less than 5μm, and the proportion of Al2O3+REM2O3 composite inclusions in Examples 1-7 to all inclusions is greater than 40%, and the proportion of inclusions with a size of 5 to 8μm to all inclusions is less than 1 / 1000, and the proportion of inclusions with a size greater than 8μm to all inclusions is less than 1 / 10000.
[0121] The average size of all inclusions in Comparative Examples 1-3 is greater than 5μm, the proportion of Al2O3+REM2O3 composite inclusions to all inclusions is far less than 40%, the proportion of inclusions with a size of 5-8μm to all inclusions is greater than 1 / 1000, and the proportion of inclusions with a size greater than 8μm to all inclusions is also greater than 1 / 10000.
[0122] In the low alloy high strength steel plates for pressure vessels of Examples 1-7, the proportion of Al2O3+REM2O3 composite inclusions to all inclusions is between 62% and 79%; the average particle size of all inclusions is between 3.69 and 4.82 μm; and the proportion of inclusions with a size of 5 to 8 μm to all inclusions is between 0.00055 and 0.00089, and the proportion of inclusions with a size greater than 8 μm to all inclusions is between 0.000039 and 0.000072.
[0123] Different from Examples 1-7, in the comparative steels of Comparative Examples 1-3, the proportion of Al2O3+REM2O3 composite inclusions to all inclusions is between 19-26%; the average particle size of all inclusions is between 5.55-6.59 μm; and the proportion of inclusions with a size of 5 to 8 μm to all inclusions is between 0.00171-0.00273, and the proportion of inclusions with a size greater than 8 μm to all inclusions is between 0.00050-0.00065.
[0124] After completing the above observation and analysis of inclusions in the steels of each embodiment and comparative example, the low alloy high strength steel plates for pressure vessels of the finished products of embodiments 1-7 and the comparative steels of comparative examples 1-3 can be sampled again, and the sample steels of embodiments 1-7 and comparative examples 1-3 obtained by the re-sampling can be subjected to mechanical property tests and low temperature impact property tests, and the specific test results are listed in the following Table 5.
[0125] The relevant detection technology solutions are as follows:
[0126] Tensile test: According to GB / T 228.1-2010 “Room temperature tensile test method for metallic materials”, the test was carried out at room temperature to obtain the yield strength and tensile strength of the steel samples of Examples 1-7 and Comparative Examples 1-3.
[0127] Impact test: According to GB / T 229-2020 “Charpy Pendulum Impact Test Method for Metallic Materials”, impact was carried out at an experimental temperature of -30°C to obtain the impact toughness of the sample steels of Examples 1-7 and Comparative Examples 1-3 at -30°C.
[0128] Table 5 lists the performance test results of the low alloy high strength steel plates for pressure vessels of Examples 1-7 and the comparative steels of Comparative Examples 1-3.
[0129] Table 5.
[0130]
[0131] In the above Table 5 of the present invention, each embodiment and comparative example has four data in the column of -30°C low temperature impact toughness, wherein the three data before " / " represent the data of three measurements respectively, and the data after " / " represent the average impact toughness.
[0132] As shown in Table 5, the yield strength of the low alloy high strength steel plates for pressure vessels of Examples 1-7 is between 451 and 518 MPa, and the tensile strength is between 581 and 633 MPa, which have relatively high strength; at the same time, the low temperature impact toughness of the low alloy high strength steel plates for pressure vessels of Examples 1-7 at -30°C is between 271 and 369 J. Although the strength of Comparative Example 1-3 is relatively high, its low temperature impact toughness at -30°C is significantly poor, which is only between 167 and 237 J.
[0133] Accordingly, high-energy-input welding can be further performed based on the obtained sample steels of Examples 1-7 and Comparative Examples 1-3. After 200 KJ / cm high-energy-input welding, the impact toughness of the welding heat-affected zone of the sample steels of each Example and Comparative Example at -30°C is measured. The specific test results are listed in the following Table 6.
[0134] Table 6.
[0135]
[0136]
[0137] Correspondingly, as shown in Table 6 above, after 200KJ / cm high-energy-input welding, the low-temperature impact toughness of the heat-affected zone of the low-alloy high-strength steel plate for pressure vessels of Examples 1-7 at -30°C is much better than that of the comparative steel of Comparative Examples 1-3. The types of inclusions in the heat-affected zone of welding were investigated by electrolytic extraction. The results show that the original Al2O3+REM2O3 composite inclusions in the steel plates of Examples 1-7 and Comparative Examples 1-3 are changed into Al2O3+REM2O3+TiN composite inclusions, but the proportion of Al2O3+REM2O3+TiN composite inclusions in the steel of Example 1-7 is much higher than that of Comparative Examples 1-3, and the overall size of the inclusions is smaller, which is mainly determined by the characteristics of the inclusions contained in the steel plates of the Examples and Comparative Examples before high-energy-input welding.
[0138] In the present invention, the low-temperature impact toughness of the heat-affected zone of the low-alloy high-strength steel plate for pressure vessels in Examples 1-7 at -30°C is between 135-230J; referring to Table 5, it can be seen that compared with the performance before high-line energy welding, the low-temperature impact toughness of the heat-affected zone of the welding is improved to a certain extent.
[0139] From the above, it can be seen that the present invention can form a large number of fine and dispersed Al2O3+REM2O3 composite inclusions in the steel by controlling the type of deoxidizer and the order of adding the deoxidizer during molten steel smelting. On the one hand, these fine composite oxides are used to hinder the growth of austenite grains in the heat affected zone at a high temperature stage; on the other hand, these Al2O3+REM2O3 composite inclusions are used as nucleation cores to absorb N and Ti elements dissolved in the metal from the surroundings of such composite inclusions, and finally form more complex Al2O3+REM2O3+TiN composite inclusions. After reducing the dissolved N element in the heat affected zone, the low-temperature impact toughness of the welding heat affected zone can be further improved, that is, the steel's resistance to high line energy welding performance is improved.
[0140] Therefore, the low-alloy high-strength steel plate for pressure vessels described in the present invention has excellent resistance to high-line energy welding. It can adopt high-line energy welding to produce pressure equipment, improve manufacturing efficiency, and improve the low-temperature impact toughness of the welding heat-affected zone. At the same time, because the steel plate also has relatively high strength, it can reduce the wall thickness of the pressure vessel while ensuring the stable and safe operation of the pressure vessel.
[0141] It should be noted that the combination of the various technical features in this case is not limited to the combination described in the claims of this case or the combination described in the specific embodiments. All technical features recorded in this case can be freely combined or combined in any way unless there is a contradiction between them.
[0142] It should also be noted that the above-listed embodiments are only specific embodiments of the present invention. Obviously, the present invention is not limited to the above embodiments, and similar changes or modifications made therewith can be directly derived or easily associated with the contents disclosed by those skilled in the art from the present invention, and all should belong to the protection scope of the present invention.
Claims
1. A low alloy high strength steel plate for a pressure vessel, characterized in that: The mass percentage of each chemical element is: C: 0.06-0.19%, Si: 0.15-0.65%, Mn: 0.30-0.80%, Cr: 2.05-3.35%, Mo: 0.40-1.25%, Als: 0.005-0.019%, Nb: 0.015-0.055%, Ti: 0.008-0.020%, REM: 0.0005-0.0020%, N: 0.0030-0.0060%, B: 0.0005-0.0025%; the balance is Fe and unavoidable impurities; It has Al2O3+REM2O3 composite inclusions, wherein the proportion of Al2O3+REM2O3 composite inclusions to all inclusions is greater than 40%, the average size of all inclusions is less than 5μm, and the proportion of inclusions with a size of 5-8μm to all inclusions is less than 1 / 1000, and the proportion of inclusions with a size greater than 8μm to all inclusions is less than 1 / 10000.
2. The low alloy high strength steel plate for pressure vessels according to claim 1, characterized in that: It also contains at least one of the following chemical elements: 0<Cu≤0.30%; 0<Ni≤0.30%.
3. The low alloy high strength steel plate for pressure vessels according to claim 1, characterized in that: Among other inevitable impurities: P ≤ 0.010%, S ≤ 0.010%.
4. The low alloy high strength steel plate for pressure vessels according to claim 1, characterized in that: The mass percentage of each chemical element satisfies at least one of the following: Ti / N: 2.40~3.50; 24×Als≥10×(24×N-7×Ti); [6+0.7714×(N-0.2916×Ti)]×10 -4 ≤B≤[25+0.7714×(N-0.2916×Ti)]×10 -4 ; 1 / 10≤REM / Als≤1 / 5; In the above formula, each element is substituted with the mass percentage of the corresponding chemical element.
5. The low alloy high strength steel plate for pressure vessels according to claim 1, characterized in that: After the steel plate is welded with a high input energy of at least 200 kJ / cm, there are fine and dispersed Al2O3+REM2O3+TiN composite inclusions in the welding heat affected zone.
6. The low alloy high strength steel plate for pressure vessels according to claim 1, characterized in that: Its yield strength is ≥450MPa, its tensile strength is ≥570MPa, and its low-temperature impact toughness at least at -30°C is ≥270J; after welding with a high line energy of at least 200kJ / cm, the low-temperature impact toughness of the welding heat affected zone at least at -30°C is ≥135J.
7. The method for manufacturing a low alloy high strength steel sheet for a pressure vessel according to any one of claims 1 to 6, characterized in that: It includes the steps of: (1) Smelting and continuous casting: Deoxidizers Si, Mn, Ti, Al and REM are added during the smelting process of the molten steel; before the molten steel is cast, pre-deoxidation is carried out in the order of Si, Mn, Ti and Al, and the oxygen level of the cast molten steel is controlled to be 0.0045-0.0085%; then, REM is used for final deoxidation, and the mass percentage of REM in the molten steel is controlled to be 0.0005-0.0020%; (2) Heating and rolling; (3) Quenching + tempering.
8. The manufacturing method according to claim 7, characterized in that: In step (1), a light reduction process is adopted at the end of solidification of the continuous casting billet, and the reduction rate is 5 to 12%.
9. The manufacturing method according to claim 7, characterized in that: In step (2), the ingot is heated to 1050-1180°C for rolling, the final rolling temperature is controlled to be greater than 900°C, and the total cumulative reduction ratio is greater than 65%.
10. The manufacturing method according to claim 9, characterized in that: In step (2), two-stage controlled rolling is adopted: in the first stage, continuous single-pass large reduction rate rolling is adopted at above 970°C, the single-pass rolling reduction rate is not less than 16%, and the total reduction rate is not less than 69%; then in the second stage, the second stage rolling is carried out at below 940°C, the single-pass rolling reduction rate is controlled to be not less than 9%, and the total reduction rate is not less than 38%.
11. The manufacturing method according to claim 7, characterized in that: In step (3), the quenching temperature is controlled to be 860-960°C, and the holding time is (1.2-2.9)×T min. After the holding time is completed, the steel plate is taken out of the furnace and water-cooled to room temperature, where T represents the thickness of the steel plate in mm.
12. The manufacturing method according to claim 7 or 11, characterized in that: In step (3), the tempering temperature is controlled to be 690-755° C., and the holding time is (2.2-3.8)×T min, where T represents the thickness of the steel plate in mm.
Citation Information
Patent Citations
Low-temperature steel for large-line energy welding with yield ratio not more than 0.85 and production method of low-temperature steel
CN103103451A
Thick high strength steel plate having excellent low temperature toughness in welding heat affected zone caused by high heat input welding
CN1946862A
Nb-Ti microalloying steel suitable for large line energy welding and smelting method therefor
CN1962916A
Manufacture method of high-strength thick steel plate capable of resisting large heat input welding
CN109321815A
Hot-rolled seamless steel tube with excellent strength and toughness and manufacturing method thereof
CN113025902A