A method for treating organic waste, a mineralized product grafted with hydroxyl groups and its application
By subjecting organic waste to microaerobic heat treatment and strong alkali solution calcination, grafted hydroxyl mineralization with a porous structure is prepared, which solves the problems of environmental pollution and resource waste caused by traditional organic waste treatment methods, achieves efficient adsorption of carbon dioxide, and achieves The goal of reducing pollution and reducing carbon emissions.
Patent Information
- Application Number
- CN202310511072.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-08
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2043-05-08
AI Technical Summary
Traditional organic waste treatment methods such as landfill and incineration have problems of environmental pollution and resource waste. There is an urgent need for an environmentally friendly pollution reduction and carbon reduction treatment method.
By subjecting organic waste to microaerobic heat treatment, mineralized matter is obtained, soaked in a strong alkaline solution and then calcined to prepare grafted hydroxyl mineralized matter with a porous structure for adsorbing harmful gases.
It realizes the resource treatment of organic waste, significantly improves the adsorption capacity of carbon dioxide, achieves the dual goals of reducing pollution and removing carbon, and the treatment process is simple and environmentally friendly.
Smart Images

Figure CN116459811B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of solid waste resource utilization, and specifically relates to a hydroxyl-grafted mineralized product and a preparation method and application thereof. Background Art
[0002] With the rapid economic development and population growth, domestic waste has also increased year by year, and most of the domestic waste is organic waste. Organic waste, also known as wet garbage, refers to waste with organic components in urban domestic waste, mainly including paper, fiber, bamboo, kitchen scraps, etc. The traditional methods of dealing with organic waste are mainly landfill and incineration. Landfilling organic waste requires a vast area, and will leach harmful chemicals into the soil, pollute groundwater, and cause the loss of nutrients in the soil. Incineration of organic waste will pollute the atmospheric environment while wasting resources. At present, there is an urgent need for an environmentally friendly method of treating organic waste to achieve the goal of reducing pollution and reducing carbon at the same time. Summary of the invention
[0003] In view of this, the present invention provides a hydroxyl-grafted mineralized product and a preparation method and application thereof. The method provided by the present invention can convert organic waste into modified mineralized products, and the modified mineralized products can be used as adsorption materials to adsorb harmful gases in waste gas, thereby achieving the goal of reducing pollution and carbon emissions.
[0004] In order to solve the above technical problems, the present invention provides a method for treating organic waste, comprising the following steps:
[0005] The organic waste is subjected to micro-oxygen heat treatment to obtain mineralized products;
[0006] The mineralized product is soaked in a strong alkaline solution and then calcined to obtain the mineralized product grafted with hydroxyl groups.
[0007] Preferably, the temperature of the micro-oxygen heat treatment is 180-230° C., the time of the micro-oxygen heat treatment is 15-24 hours, and the oxygen concentration in the micro-oxygen heat treatment environment is 0.1-1 ml / L.
[0008] Preferably, before the soaking, the method further comprises: grinding the mineralized material; the average particle size of the ground mineralized material obtained by the grinding is 100 to 200 meshes.
[0009] Preferably, the strong alkali solution comprises sodium hydroxide solution or potassium hydroxide solution; the molar concentration of the strong alkali solution is 1 to 5 mol / L; and the mass ratio of the strong alkali solution to the mineralized material is 10:0.5 to 1.
[0010] Preferably, the soaking time is 5 to 8 hours.
[0011] Preferably, before the calcination, the method further comprises: subjecting the alkali-leached mineralized product obtained by the immersion to an aging treatment;
[0012] The temperature of the aging treatment is 75 to 85° C., and the time of the aging treatment is 10 to 20 hours.
[0013] Preferably, the calcination is carried out under a protective atmosphere;
[0014] The calcination temperature is 350-500° C., and the calcination time is 3-7 hours.
[0015] The present invention also provides a grafted hydroxyl mineralized product prepared by the method described in the above technical solution, wherein the grafted hydroxyl mineralized product has a porous structure, and the porosity of the grafted hydroxyl mineralized product is 30-50%;
[0016] The content of hydroxyl groups in the mineralized product grafted with hydroxyl groups is 1 to 13%.
[0017] The present invention also provides the use of the mineralized product grafted with hydroxyl groups described in the above technical solution in the adsorption of harmful gases.
[0018] Preferably, the harmful gas includes carbon dioxide or organic volatile gas.
[0019] The present invention provides a method for treating organic waste, comprising the following steps: subjecting the organic waste to micro-oxygen heat treatment to obtain a mineralized product; and calcining the mineralized product after soaking it in a strong alkaline solution to obtain a mineralized product grafted with hydroxyl groups. The present invention subjecting the organic waste to micro-oxygen treatment to obtain a mineralized product containing a pore structure, and calcining the product after introducing hydroxyl groups into the mineralized product to obtain a porous mineralized product grafted with hydroxyl groups. The mineralized product grafted with hydroxyl groups obtained according to the method of the present invention can effectively adsorb harmful gases, such as carbon dioxide. The present invention processes organic waste as a resource and can adsorb carbon dioxide, achieving the dual goals of reducing pollution and removing carbon, and having significant economic and environmental benefits. The method provided by the present invention is simple, easy to operate, and will not pollute the environment. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 This is a graph showing the carbon dioxide adsorption-desorption curve of the grafted hydroxyl mineralized product prepared in Example 1. DETAILED DESCRIPTION
[0021] The present invention provides a method for treating organic waste, comprising the following steps:
[0022] The organic waste is subjected to micro-oxygen heat treatment to obtain mineralized products;
[0023] The mineralized product is soaked in a strong alkaline solution and then calcined to obtain the mineralized product grafted with hydroxyl groups.
[0024] The present invention conducts micro-oxygen heat treatment on organic waste to obtain mineralized products. In the present invention, the organic waste preferably includes one or more of plastic, grease, waste paper, kitchen waste, straw, leather, rubber, fiber, and wood. In the present invention, the temperature of the micro-oxygen heat treatment is preferably 180-230°C, more preferably 190-220°C; the time of the micro-oxygen heat treatment is preferably 15-24h, more preferably 15-20h; the oxygen concentration in the environment of the micro-oxygen heat treatment is preferably 0.1-1ml / L, more preferably 0.3-0.6ml / L.
[0025] The present invention can slowly oxidize organic matter to release energy through micro-oxygen treatment, so that organic waste can be slowly mineralized and the specific surface area of the mineralized product can be increased. If the oxidation is carried out in an environment with a large amount of oxygen, the organic waste will burn, release heat violently, and the system temperature will increase significantly, so that the material mineralization process will become faster and the specific surface area of the mineralized product will become smaller.
[0026] In the present invention, when the oxygen concentration in the micro-oxygen heat treatment is lower than 0.1 ml / L, the oxidation reaction cannot be carried out, and the oxidation reaction can only be carried out by raising the temperature to above 350°C; when the oxygen concentration is higher than 1 ml / L, the treatment process will lead to combustion, and the normal temperature after combustion will reach above 400°C; the above two reaction processes will produce dioxin carcinogens, resulting in a significant increase in the overall reaction cost. In addition, the anoxic treatment product contains a large amount of tar, and also exists in an amorphous state, with low compressive strength; after the combustion treatment, the product will agglomerate, resulting in a significant reduction in specific surface area.
[0027] After obtaining the mineralized product, the present invention soaks the mineralized product in a strong alkaline solution and then calcines it to obtain a mineralized product grafted with hydroxyl groups. In the present invention, the soaking preferably also includes: grinding the mineralized product. In the present invention, the average particle size of the ground mineralized product obtained by grinding is preferably 100 to 200 meshes, more preferably 130 to 150 meshes. The present invention has no special limitation on the grinding method, as long as the desired particle size can be achieved.
[0028] In the present invention, the strong alkali solution preferably includes sodium hydroxide solution or potassium hydroxide solution, more preferably sodium hydroxide solution. In the present invention, the molar concentration of the strong alkali solution is preferably 1-5 mol / L, more preferably 1-3 mol / L. In the present invention, the mass ratio of the strong alkali solution to the mineralized material is preferably 10:0.5-1, more preferably 10:0.6-0.8. In the present invention, the soaking time is preferably 5-8h, more preferably 6-7h.
[0029] The present invention preferably filters the soaking system to obtain the alkali-leached mineralized product.
[0030] The invention adsorbs hydroxide ions into the pores of the mineralized material through soaking.
[0031] In the present invention, the calcination step preferably further comprises: subjecting the alkali-leached mineralized product obtained by soaking to an aging treatment. In the present invention, the aging treatment temperature is preferably 75 to 85° C., more preferably 78 to 80° C.; the aging treatment time is preferably 10 to 20 hours, more preferably 12 to 15 hours.
[0032] The invention can stabilize the hydroxide ions on the mineralized material through aging treatment, thereby enhancing the stability of the hydroxide ions.
[0033] In the present invention, the calcination is preferably carried out under a protective atmosphere; the protective atmosphere preferably includes nitrogen or argon, more preferably nitrogen.
[0034] In the present invention, the calcination temperature is preferably 350-500° C., more preferably 400-450° C.; the calcination time is preferably 3-7 h, more preferably 5-6 h.
[0035] The invention can remove moisture from the mineralized product through calcination, and at the same time make the hydroxide ions combine with the mineralized product in the form of hydroxyl groups to form the mineralized product grafted with hydroxyl groups.
[0036] The present invention also provides a grafted hydroxyl mineral prepared by the method described in the above technical solution, wherein the grafted hydroxyl mineral has a porous structure, and the porosity of the grafted hydroxyl mineral is 30-50%, preferably 48-50%. In the present invention, the porous structure is preferably sponge-like. In the present invention, the content of hydroxyl in the grafted hydroxyl mineral is 1-13%, preferably 3-5.41%, and more preferably 2-4%.
[0037] In the present invention, the mineralized product of grafted hydroxyl groups preferably comprises the following chemical components: SiO2, CaAl2Si2O8, Al2SiO5, CaCO3, CaO and ZnMn2O4. In the present invention, the contents of SiO2, CaAl2Si2O8, Al2SiO5, CaCO3, CaO and ZnMn2O4 in the mineralized product of grafted hydroxyl groups are determined by the composition of organic waste.
[0038] The present invention also provides the use of the mineralized product grafted with hydroxyl groups in the above technical solution in the adsorption of harmful gases. In the present invention, the harmful gas preferably includes carbon dioxide or organic volatile gas, more preferably carbon dioxide.
[0039] In order to further illustrate the present invention, the technical solutions provided by the present invention are described in detail below in conjunction with embodiments, but they should not be construed as limiting the protection scope of the present invention.
[0040] Example 1
[0041] Take plastic, grease, waste paper, kitchen waste, straw, leather, rubber, fiber and wood in domestic waste as organic waste raw materials;
[0042] The organic waste is subjected to micro-oxygen heat treatment at a temperature of 230°C and an oxygen concentration of 0.3 ml / L for 15 hours to obtain mineralized products;
[0043] The mineralized material is ground and sieved to obtain mineralized particles with an average particle size of 150 meshes, and the mineralized particles are soaked in a NaOH solution with a molar concentration of 1 mol / L (the mass ratio of the mineralized particles to the NaOH solution is 10:0.8) for 6 hours and then filtered to obtain the mineralized material soaked in the sodium hydroxide solution;
[0044] The mineralized product soaked in sodium hydroxide solution was aged at 80° C. for 14 h and then calcined at 450° C. for 5 h in a nitrogen atmosphere to obtain a mineralized product grafted with hydroxyl groups.
[0045] Example 2
[0046] Take plastic, grease, waste paper, kitchen waste, straw, leather, rubber, fiber and wood in domestic waste as organic waste raw materials;
[0047] The organic waste is subjected to micro-oxygen heat treatment at a temperature of 220°C and an oxygen concentration of 0.5 ml / L for 20 hours to obtain mineralized products;
[0048] The mineralized material is ground and sieved to obtain mineralized particles with an average particle size of 150 meshes, and the mineralized particles are soaked in a NaOH solution with a molar concentration of 2 mol / L (the mass ratio of the mineralized particles to the NaOH solution is 10:0.7) for 5.5 hours and then filtered to obtain the mineralized material soaked in the sodium hydroxide solution;
[0049] The mineralized product soaked in sodium hydroxide solution was aged at 80° C. for 12 h and then calcined at 420° C. for 6 h in a nitrogen atmosphere to obtain a mineralized product grafted with hydroxyl groups.
[0050] Example 3
[0051] Take plastic, grease, waste paper, kitchen waste, straw, leather, rubber, fiber and wood in domestic waste as organic waste raw materials;
[0052] The organic waste is subjected to micro-oxygen heat treatment at a temperature of 200°C and an oxygen concentration of 0.6 ml / L for 24 hours to obtain mineralized products;
[0053] The mineralized material is ground and sieved to obtain mineralized particles with an average particle size of 150 meshes, and the mineralized particles are soaked in a NaOH solution with a molar concentration of 5 mol / L (the mass ratio of the mineralized particles to the NaOH solution is 10:1) for 5 hours and then filtered to obtain the mineralized material soaked in the sodium hydroxide solution;
[0054] The mineralized product soaked in sodium hydroxide solution was aged at 80° C. for 15 h and then calcined at 400° C. for 7 h in a nitrogen atmosphere to obtain a mineralized product grafted with hydroxyl groups.
[0055] Comparative Example 1
[0056] Take plastic, grease, waste paper, kitchen waste, straw, leather, rubber, fiber and wood in domestic waste as organic waste raw materials;
[0057] The organic waste was subjected to micro-oxygen heat treatment at a temperature of 250°C and an oxygen concentration of 0.05 ml / L for 24 hours, but no mineralized product was obtained.
[0058] Comparative Example 2
[0059] The mineralized material was prepared according to the method of Example 1, except that it was not soaked in a strong alkaline solution.
[0060] The porosity and specific surface area of the mineralized products grafted with hydroxyl groups prepared in Examples 1 to 3 and Comparative Examples 1 to 2 were analyzed by CO2 BET. The results are listed in Table 1.
[0061] Table 1 Performance parameters of the mineralized products of grafted hydroxyl groups prepared in Examples 1 to 3 and Comparative Examples 1 to 2
[0062]
[0063] It can be seen from Table 1 that the mineralized product grafted with hydroxyl groups obtained by the method provided by the present invention has a higher porosity and a larger specific surface area.
[0064] The adsorption performance of the mineralized products of grafted hydroxyl groups prepared in Examples 1 to 3 and Comparative Example 1 was analyzed by BET, and the results are listed in Table 2. The carbon dioxide adsorption-desorption curve of the mineralized products of grafted hydroxyl groups prepared in Example 1 is shown in Table 2. Figure 1 shown.
[0065] Table 2 Adsorption properties of the mineralized products with grafted hydroxyl groups prepared in Examples 1 to 3 and Comparative Example 2
[0066]
[0067] According to Table 2 and Figure 1 It can be seen that the mineralized product with grafted hydroxyl groups provided by the present invention has good adsorption performance for carbon dioxide.
[0068] Although the above embodiment describes the present invention in detail, it is only a part of the embodiments of the present invention, not all of the embodiments. People can also obtain other embodiments based on this embodiment without creativity, and these embodiments all fall within the protection scope of the present invention.
Claims
1. A method for treating organic waste, comprising the following steps: The organic waste is subjected to micro-oxygen heat treatment to obtain mineralized products; the temperature of the micro-oxygen heat treatment is 180-230° C., the time of the micro-oxygen heat treatment is 15-24 hours, and the oxygen concentration in the micro-oxygen heat treatment environment is 0.1-1 ml / L; The mineralized product is soaked in a strong alkaline solution and then calcined to obtain the mineralized product grafted with hydroxyl groups.
2. The method according to claim 1, characterized in that: Before the soaking, the method further comprises: grinding the mineralized material; the average particle size of the ground mineralized material obtained by the grinding is 100 to 200 meshes.
3. The method according to claim 1 or 2, characterized in that: The strong alkali solution includes sodium hydroxide solution or potassium hydroxide solution; the molar concentration of the strong alkali solution is 1-5 mol / L; the mass ratio of the strong alkali solution to the mineralized material is 10:0.5-1.
4. The method according to claim 3, characterized in that: The soaking time is 5 to 8 hours.
5. The method according to claim 1, characterized in that: Before the calcination, the method further comprises: subjecting the alkali-leached mineralized product obtained by the immersion to an aging treatment.
6. The method according to claim 5, characterized in that: The temperature of the aging treatment is 75-85° C., and the time of the aging treatment is 10-20 hours.
7. The method according to claim 1, characterized in that: The calcination is carried out under a protective atmosphere; The calcination temperature is 350-500° C., and the calcination time is 3-7 hours.
8. A hydroxyl-grafted mineral prepared according to the method of any one of claims 1 to 7, wherein the hydroxyl-grafted mineral has a porous structure and a porosity of 30 to 50%; The content of hydroxyl groups in the mineralized product grafted with hydroxyl groups is 1 to 13%.
9. Use of the mineralized product grafted with hydroxyl groups according to claim 8 in the adsorption of harmful gases.
10. The use according to claim 9, characterized in that: The harmful gas includes carbon dioxide or organic volatile gas.