A method for removing carbon from waste silicone contacts and waste pulp residues

After vacuum drying and vibration mill treatment, low-temperature and low-oxygen potential roasting in a mixed atmosphere of nitrogen and air solves the problem of carbon removal in organic silicon waste contacts and waste slurry residues, and achieves efficient carbon removal and silicon powder removal. Optimization achieves the goals of resource reuse and environmental protection.

CN116462199BActive Publication Date: 2024-10-22KUNMING UNIV OF SCI & TECH
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202310510378.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-05-08
Publication Date
2024-10-22
Estimated Expiration
2043-05-08

AI Technical Summary

Technical Problem

The existing technology is difficult to effectively remove carbon when processing organic silicon waste contacts and waste slurry residues, resulting in environmental pollution and resource waste. The efficiency of extracting silicon powder is low, and the process is complex and requires high equipment.

Method used

After vacuum drying and vibration grinding, low-temperature and low-oxygen potential oxidation roasting is performed in a mixed atmosphere of nitrogen and air. The temperature is controlled at 300-500°C and the time is 1-8 hours to remove the organic silicon waste contacts and waste slurry. The carbon in the slag slows down the oxidation rate of silicon and improves the carbon removal rate.

Benefits of technology

The carbon content has been significantly reduced, and the performance of silicon powder has been optimized. It can be used as a high-quality silicon smelting raw material and silicon-based inoculant to achieve the purpose of waste reuse, with a carbon removal rate of 98.23% to 98.67%.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116462199B_ABST
    Figure CN116462199B_ABST
Patent Text Reader

Abstract

The present invention discloses a method for removing carbon from waste organosilicon contacts and waste pulp residues, which is characterized by comprising the following steps: vacuum drying the waste organosilicon contacts and waste pulp residues, grinding them with a vibration mill, and then passing through a 50-150 mesh screen; placing the ground samples in a mixed atmosphere of nitrogen and air, and performing oxidation roasting at 300-500°C for 1-8 hours to obtain silicon powder with a low carbon content. The present invention fully volatilizes and removes the organic carbon in the waste organosilicon contacts and waste pulp residues through roasting. In order to control the oxidation of the metal silicon powder, low-temperature oxidation roasting, a shorter roasting time, and a controlled oxidizing atmosphere are selected to react the inorganic carbon in the material with oxygen to generate carbon monoxide or carbon dioxide gas to escape, thereby reducing silicon oxidation and increasing the removal rate of impurity carbon; the silicon powder obtained by the process has a lower carbon content and better performance, and can be used as a raw material and silicon-based inoculant for silicon smelting enterprises to achieve the purpose of waste recycling.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of resource utilization of waste organosilicon slurry and waste contacts, and in particular relates to a method for removing carbon from waste organosilicon contacts and waste slurry. Background Art

[0002] At present, the production of organosilicon monomers at home and abroad generally adopts the direct method to synthesize methylchlorosilane, and a large amount of waste slurry and waste contacts will be generated during the production process. The waste slurry is mainly composed of high boiling points and unreacted silicon powder, copper powder and a small amount of carbon, with a solid content of about 25%; the waste contacts mainly contain about 70-75% silicon (mainly elemental silicon), about 5-10% copper, and 1-10% carbon.

[0003] Many companies extract copper from waste contacts and waste slag slurry through ammonia leaching, reduction or other methods. The above methods only extract 10-15% of the copper, and a large amount of silicon powder with recycling value is not utilized as a resource. Waste contacts and waste slag slurry contain 60-70% silicon powder, 3.28-15.83% carbon, 2-3% iron, 9-10% chlorine and a small amount of other impurities. The removal rate of chlorine through water washing is 90%. Companies generally landfill or incinerate the above waste slag. Direct landfill or incineration will have a great impact on the environment. Incineration will produce a large amount of toxic gases and cause secondary pollution; landfill will take up a large space, and the precipitated substances will cause soil and groundwater pollution. Chinese patent CN114349010A discloses a method for removing carbon from waste silicon powder after copper extraction, wherein OP series emulsifiers, surfactants, dibutyl esters and water are added to the waste silicon powder after copper extraction, stirred and allowed to settle, and the lower precipitate is washed and dried to reduce the carbon content from 3-6% to 1%. The operation process is complicated and will also bring a series of waste liquid treatment problems. Chinese patent CN115181998A discloses a method for recovering high-purity silicon powder from waste organic silicon contacts, wherein silicon powder with a purity of about 98% is obtained by adding sulfuric acid and an adjusting agent for oxidation acid leaching, washing and filtering the leached residue, and then neutralizing. The process of this method is long, and the acid leaching has the defects of high equipment requirements and environmental pollution.

[0004] Therefore, in order to solve the above problems, this paper proposes a method for removing carbon from waste silicone contacts and waste pulp. Summary of the invention

[0005] In order to solve the above technical problems, the present invention designs a method for removing carbon from waste silicone contacts and waste pulp residues.

[0006] In order to achieve the above technical effects, the present invention is implemented by the following technical scheme: a method for removing carbon from waste silicone contacts and waste pulp residues, characterized in that it comprises the following steps:

[0007] Step 1: vacuum dry the waste silicone contact body and waste pulp residue, grind them with a vibration mill and pass them through a 50-150 mesh screen;

[0008] Step 2: The ground sample is placed in a mixed atmosphere of nitrogen and air, and oxidatively calcined at 300-500°C for 1-8 hours to obtain silicon powder with a low carbon content.

[0009] Furthermore, the sieve described in Step 1 is 100 mesh.

[0010] Furthermore, the oxidation roasting temperature described in Step 2 is 500° C. and the time is 5 h.

[0011] Furthermore, the volume ratio of nitrogen to air in the mixed atmosphere of Step 2 is 1:3 to 1:5.

[0012] Furthermore, the volume ratio of nitrogen to air in the mixed atmosphere is 1:4.

[0013] The beneficial effects of the present invention are:

[0014] The method for removing carbon from waste organosilicon contacts and waste slurry residues described in the present invention fully volatilizes and removes the organic carbon in the waste organosilicon contacts and waste slurry residues through roasting. In order to control the oxidation of metallic silicon powder, low-temperature and low-oxygen potential roasting is selected to slow down the oxidation rate of silicon. A sufficiently long roasting time is used to ensure that the inorganic carbon in the material reacts with oxygen to generate carbon monoxide or carbon dioxide gas to escape, thereby reducing silicon oxidation and increasing the removal rate of impurity carbon. The silicon powder obtained by this process has a lower carbon content and better performance, and can be used as a raw material and silicon-based inoculant for silicon smelting enterprises to achieve the purpose of waste recycling. BRIEF DESCRIPTION OF THE DRAWINGS

[0015] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for describing the embodiments are briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.

[0016] Figure 1 It is a schematic flow diagram of the method for removing carbon from waste organic silicon contacts and waste pulp residues of the present invention;

[0017] Figure 2 The infrared spectrum analysis of the waste silicone contact body and waste pulp residue after drying and grinding of the present invention;

[0018] Figure 3 This is the infrared spectrum analysis of the low carbon content silicon powder obtained after roasting and decarbonization in the embodiment of the present invention. DETAILED DESCRIPTION

[0019] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0020] Example 1

[0021] A method for removing carbon from waste silicone contacts and waste pulp residues, the specific steps are as follows:

[0022] (1) Take a certain amount of waste silicone contacts and waste pulp residue and dry them in a vacuum drying oven, and grind the dried samples in a vibration mill until all the materials pass through a 100-mesh sieve;

[0023] (2) taking 20 g of the sample prepared in step (1) and placing it in a corundum boat, placing the corundum boat in a horizontal resistance furnace, adjusting the roasting temperature to 500° C., and heating in a mixed atmosphere of nitrogen and air with a volume ratio of 1:4 for 3 h;

[0024] (3) After the temperature naturally cooled to room temperature, the sample was taken out to detect the carbon content, wherein the removal rate of impurity carbon reached 98.23%.

[0025] Example 2

[0026] A method for removing carbon from waste silicone contacts and waste pulp residues, the specific steps are as follows:

[0027] (1) Take a certain amount of waste silicone contacts and waste pulp residue and dry them in a vacuum drying oven, and grind the dried samples in a vibration mill until all the materials pass through a 100-mesh sieve;

[0028] (2) taking 20 g of the sample prepared in step (1) and placing it in a corundum boat, placing the corundum boat in a horizontal resistance furnace, adjusting the roasting temperature to 500° C., and heating in a mixed atmosphere of nitrogen and air with a volume ratio of 1:4 for 5 h;

[0029] (3) After the temperature naturally cooled to room temperature, the sample was taken out to detect the carbon content, wherein the removal rate of impurity carbon reached 99.55%.

[0030] Example 3

[0031] A method for removing carbon from waste silicone contacts and waste pulp residues, the specific steps are as follows:

[0032] (1) Take a certain amount of waste silicone contacts and waste pulp residue and dry them in a vacuum drying oven, and crush and grind the dried samples in a vibration mill until all the materials pass through a 100-mesh sieve;

[0033] (2) taking 20 g of the sample prepared in step (1) and placing it in a corundum boat, placing the corundum boat in a horizontal resistance furnace, adjusting the roasting temperature to 500° C., and heating in a mixed atmosphere of nitrogen and air with a volume ratio of 1:4 for 1 h;

[0034] (3) After the temperature naturally cooled to room temperature, the sample was taken out to detect the carbon content, wherein the removal rate of impurity carbon reached 83.539%.

[0035] Example 4

[0036] A method for removing carbon from waste silicone contacts and waste pulp residues, the specific steps are as follows:

[0037] (1) Take a certain amount of waste silicone contacts and waste pulp residue and dry them in a vacuum drying oven, and crush and grind the dried samples in a vibration mill until all the materials pass through a 100-mesh sieve;

[0038] (2) taking 20 g of the sample prepared in step (1) and placing it in a corundum boat, placing the corundum boat in a horizontal resistance furnace, adjusting the roasting temperature to 450° C., and heating for 2 h in a mixed atmosphere of nitrogen and air with a volume ratio of 1:3;

[0039] (3) After the temperature naturally cooled to room temperature, the sample was taken out to detect the carbon content, wherein the removal rate of impurity carbon reached 88.50%.

[0040] Example 5

[0041] A method for removing carbon from waste silicone contacts and waste pulp residues, the specific steps are as follows:

[0042] (1) Take a certain amount of waste silicone contacts and waste pulp residue and dry them in a vacuum drying oven, and crush and grind the dried samples in a vibration mill until all the materials pass through a 100-mesh sieve;

[0043] (2) taking 20 g of the sample of step (1) and putting it into a corundum boat, and placing the corundum boat in a horizontal resistance furnace, adjusting the roasting temperature to 450° C., and heating in a mixed atmosphere of nitrogen and air with a volume ratio of 1:4 for 3 h;

[0044] (3) After the temperature naturally cooled to room temperature, the sample was taken out to detect the carbon content, wherein the removal rate of impurity carbon reached 94.06%.

[0045] Example 6

[0046] A method for removing carbon from waste silicone contacts and waste pulp residues, the specific steps are as follows:

[0047] (1) Take a certain amount of waste silicone contacts and waste pulp residue and dry them in a vacuum drying oven, and crush and grind the dried samples in a vibration mill until all the materials pass through a 100-mesh sieve;

[0048] (2) taking 20 g of the sample of step (1) and putting it into a corundum boat, and placing the corundum boat in a horizontal resistance furnace, adjusting the roasting temperature to 450° C., and heating in a mixed atmosphere of nitrogen and air with a volume ratio of 1:4 for 6 h;

[0049] (3) After the temperature naturally cooled to room temperature, the sample was taken out to detect the carbon content, wherein the removal rate of impurity carbon reached 98.92%.

[0050] Example 7

[0051] A method for removing carbon from waste silicone contacts and waste pulp residues, the specific steps are as follows:

[0052] (1) Take a certain amount of waste silicone contacts and waste pulp residue and dry them in a vacuum drying oven, and crush and grind the dried samples in a vibration mill until all the materials pass through a 100-mesh sieve;

[0053] (2) taking 20 g of the sample prepared in step (1) and placing it in a corundum boat, placing the corundum boat in a horizontal resistance furnace, adjusting the roasting temperature to 400° C., and heating in a mixed atmosphere of nitrogen and air with a volume ratio of 1:4 for 3 h;

[0054] (3) After the temperature naturally cooled to room temperature, the sample was taken out to detect the carbon content, wherein the removal rate of impurity carbon reached 81.80%.

[0055] Example 8

[0056] A method for removing carbon from waste silicone contacts and waste pulp residues, the specific steps are as follows:

[0057] (1) Take a certain amount of waste silicone contacts and waste pulp residue and dry them in a vacuum drying oven, and crush and grind the dried samples in a vibration mill until all the materials pass through a 100-mesh sieve;

[0058] (2) taking 20 g of the sample prepared in step (1) and placing it in a corundum boat, placing the corundum boat in a horizontal resistance furnace, adjusting the roasting temperature to 400° C., and heating in a mixed atmosphere of nitrogen and air with a volume ratio of 1:4 for 7 h;

[0059] (3) After the temperature naturally cooled to room temperature, the sample was taken out to detect the carbon content, wherein the removal rate of impurity carbon reached 98.67%.

[0060] Example 9

[0061] A method for removing carbon from waste silicone contacts and waste pulp residues, the specific steps are as follows:

[0062] (1) Take a certain amount of waste silicone contacts and waste pulp residue and dry them in a vacuum drying oven, and crush and grind the dried samples in a vibration mill until all the materials pass through a 100-mesh sieve;

[0063] (2) taking 20 g of the sample prepared in step (1) and placing it in a corundum boat, placing the corundum boat in a horizontal resistance furnace, adjusting the roasting temperature to 350° C., and heating in a mixed atmosphere of nitrogen and air with a volume ratio of 1:5 for 8 h;

[0064] (3) After the temperature naturally cooled to room temperature, the sample was taken out to detect the carbon content, wherein the removal rate of impurity carbon reached 97.53%.

[0065] Example 10

[0066] A method for removing carbon from waste silicone contacts and waste pulp residues, the specific steps are as follows:

[0067] (1) Take a certain amount of waste silicone contacts and waste pulp residue and dry them in a vacuum drying oven, and crush and grind the dried samples in a vibration mill until all the materials pass through a 100-mesh sieve;

[0068] (2) taking 20 g of the sample prepared in step (1) and placing it in a corundum boat, placing the corundum boat in a horizontal resistance furnace, adjusting the roasting temperature to 300° C., and heating in a mixed atmosphere of nitrogen and air with a volume ratio of 1:4 for 3 h;

[0069] (3) After the temperature naturally cooled to room temperature, the sample was taken out to detect the carbon content, wherein the removal rate of impurity carbon reached 45.16%.

[0070] Embodiment 11

[0071] By the attached Figure 2 and attached Figure 3 It can be clearly seen that Figure 2 Middle 2961.69cm -1 Corresponding to the characteristic peak of CH, 1260.2cm -1 The corresponding Si-(CH 3 ) 2 The characteristic absorption peaks disappear significantly after low-temperature calcination and carbon removal, indicating that low-temperature and low-oxygen potential calcination can effectively remove organic carbon and inorganic carbon from waste silicone contacts and waste pulp residues.

Claims

1. A method for removing carbon from waste silicone contacts and waste pulp, characterized in that: It consists of the following steps: (1): The waste silicone contacts and waste pulp are vacuum dried, ground with a vibration mill, and then passed through a 50-150 mesh screen; (2) The ground sample is placed in a mixed atmosphere of nitrogen and air in a volume ratio of nitrogen to air = 1:3 to 1:5, and oxidatively calcined at 300 to 500° C. for 1 to 8 hours to obtain silicon powder with a low carbon content.

2. The method for removing carbon from waste silicone contacts and waste pulp according to claim 1, characterized in that: The sieve described in (1) is 100 mesh.

3. The method for removing carbon from waste organic silicon contacts and waste pulp according to claim 1, characterized in that: The oxidation roasting temperature described in (2) is 500°C and the time is 5 hours.

4. The method for removing carbon from waste silicone contacts and waste pulp according to claim 1, characterized in that: The volume ratio of nitrogen to air in the mixed atmosphere is 1:4.

Citation Information

Patent Citations

  • Method for removing carbon from waste silicon powder after copper extraction

    CN114349010A

  • Method for recovering copper and high-purity silicon powder from organic silicon waste contact

    CN115181998A

  • Catalyst for low-temperature synthesis of methanol and preparation method

    CN102773102A

  • Organic silicon waste contact recovery method

    CN104843721A