Preparation and application of modified graphene oxide / polyvinylidene fluoride / carboxymethyl polyphenylene sulfide composite material
By preparing composite materials of modified graphene oxide, polyvinylidene fluoride and carboxylated polyphenylene sulfide, a coating with high specific surface area and strong interfacial interaction is formed, which solves the problem of poor anti-corrosion performance of existing composite materials and achieves It has significant anti-corrosion and improved mechanical properties and is suitable for metal surface protection in marine environments.
Patent Information
- Application Number
- CN202310447566.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-24
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2043-04-24
AI Technical Summary
The existing composite materials prepared by mixing polyphenylene sulfide and polyvinylidene fluoride have poor anti-corrosion properties, and the coating function is single, making it difficult to achieve good results in terms of surface morphology, wettability, hydrophobicity, thermal stability and anti-corrosion properties. Significant improvement.
Using the preparation method of modified graphene oxide, polyvinylidene fluoride and carboxylated polyphenylene sulfide composite materials, through ultrasonic dispersion and spraying technology, a composite coating with high specific surface area and strong interface interaction is formed to enhance anti-corrosion performance .
The anti-corrosion performance, high temperature resistance and mechanical properties of the composite coating are significantly improved. It can exist stably in a marine environment with high humidity and salt content, and is suitable for the protection of metal surfaces.
Smart Images

Figure CN116462968B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of polyphenylene sulfide composite materials, and in particular to the preparation and application of a modified graphene oxide / polyvinylidene fluoride / carboxymethyl polyphenylene sulfide composite material. Background Art
[0002] Polyphenylene sulfide (PPS) is a cost-effective thermoplastic engineering polymer with high thermal stability, good mechanical properties, chemical resistance, high temperature resistance, radiation resistance, flame retardancy and high dimensional stability. The outstanding characteristics of PPS make it widely used in various fields such as chemistry, industrial equipment, and marine environment. The main chain of polyphenylene sulfide is composed of rigid benzene rings and flexible sulfide bonds, so it has the characteristics of both rigidity and flexibility. Its microscopic morphology includes lamellar, hollow spherical, rod-shaped, and flower-shaped structures. Since polyphenylene sulfide has good compatibility, it can be modified by alloying modification, physical blending, and chemical grafting to obtain composite materials with excellent performance.
[0003] Polyvinylidene fluoride (PVDF) is a thermoplastic polymer commonly used in the manufacture of membrane polymer materials. It has good thermal stability, fire resistance, excellent chemical resistance and high mechanical properties. Therefore, PVDF is widely used in many fields such as sensors, chemical thermal acid, biomedicine and high temperature.
[0004] A large number of studies have shown that the defects in a single coating can be filled by blending nanofillers with similar viscosity or functionalization, and the corrosion resistance of the coating can be effectively improved by delaying the diffusion path of the corrosive medium in the coating and increasing the interfacial adhesion inside the coating. However, the corrosion resistance of the composite material prepared by directly mixing polyphenylene sulfide and polyvinylidene fluoride is still not high. The coating prepared by the composite of modified graphene oxide, polyvinylidene fluoride and carboxylated polyphenylene sulfide in the present invention has been greatly improved in terms of surface morphology, wettability, hydrophobicity, thermal stability and corrosion resistance. Summary of the invention
[0005] The purpose of the present invention is to provide a preparation and application of a modified graphene oxide / polyvinylidene fluoride / carboxymethyl polyphenylene sulfide composite material to solve the problem that the above-mentioned coating has a relatively single function and poor anti-corrosion performance.
[0006] To achieve the above object, the first aspect of the present invention provides a method for preparing a modified graphene oxide / polyvinylidene fluoride / carboxymethyl polyphenylene sulfide composite material, comprising the following steps:
[0007] (1) Preparation of modified graphene oxide
[0008] Using graphene oxide and octadecylamine as raw materials and ethanol as solvent, the modified graphene oxide is obtained by centrifugation, washing and vacuum drying after ultrasonic treatment; the modified graphene is recorded as GO-ODA;
[0009] (2) Preparation of carboxylated polyphenylene sulfide
[0010] With anhydrous sodium sulfide, p-dichlorobenzene and 2,5-dichlorobenzoic acid as raw materials, N-methylpyrrolidone as solvent, isopropyl titanate as catalyst, nitrogen as protective gas, react at 260-280°C for 1.5-2.5h in an alkaline environment, wash, filter and dry to obtain carboxylated polyphenylene sulfide; carboxylated polyphenylene sulfide is recorded as PPS-COOH;
[0011] (3) Preparation of modified graphene oxide / polyvinylidene fluoride / carboxylated polyphenylene sulfide composites
[0012] The modified graphene oxide, polyvinylidene fluoride and carboxylated polyphenylene sulfide were evenly dispersed by ultrasonic in ethanol, filtered, washed and freeze-dried to obtain a modified graphene oxide / polyvinylidene fluoride / carboxylated polyphenylene sulfide composite material; recorded as GO-ODA / PVDF / PPS.
[0013] Preferably, the preparation process of graphene oxide in step (1) is as follows: first, take expanded graphite and disperse it evenly in DMF solvent, ultrasonically exfoliate it for 24 hours, filter, wash and dry the obtained product to obtain liquid-phase ultrasonically exfoliated graphite flakes, take 1 g of it and add it to 120 mL of 0°C mixed acid, maintain the temperature of ice water bath and stir, and slowly add potassium permanganate, continue stirring and react at 50°C for 12 hours, after the reaction is completed, add 200 mL of ice water and 5 mL of hydrogen peroxide solution, observe that the color of the solution gradually changes from purple-red to golden yellow, separate, filter, wash and dry the solution to obtain graphene oxide.
[0014] Preferably, the volume mass ratio of DMF to expanded graphite is 1 L / g; the mixed acid includes a concentrated sulfuric acid solution and a concentrated phosphoric acid solution in a mass ratio of 3:1, the volume mass of the concentrated sulfuric acid solution is 50 mL / g, and the volume mass of the concentrated phosphoric acid solution is 30 mL / g; the mass ratio of graphite flakes to potassium permanganate is 1:9; and the mass concentration of the H2O2 solution is 30%.
[0015] Preferably, in step (1), the mass ratio of graphene oxide to octadecylamine is 1:4; freeze drying is performed at -60 to -70°C for 12 to 13 hours, and centrifugation is performed at 6000 rpm; vacuum drying is performed at 110 to 130°C for 3 to 5 hours.
[0016] Preferably, in step (2), the mass ratio of 2,5-dichlorobenzoic acid to anhydrous sodium sulfide is 1:15-1:16, the mass ratio of 2,5-dichlorobenzoic acid to p-dichlorobenzene is 1:10-1:12, and the mass ratio of 2,5-dichlorobenzoic acid to isopropyl titanate is 25:1-30:1.
[0017] Preferably, in step (3), the amount of modified graphene oxide added is 2% to 6% of the mass of carboxylated polyphenylene sulfide.
[0018] Preferably, in step (3), the mass ratio of modified graphene oxide to polyvinylidene fluoride is 2:6 to 6:2.
[0019] Preferably, in step (3), freeze drying is performed at -50 to -60°C for 12 to 24 hours.
[0020] The second aspect of the present invention provides an application of a modified graphene oxide / polyvinylidene fluoride / carboxymethyl polyphenylene sulfide composite material, and an application of the modified graphene oxide / polyvinylidene fluoride / carboxymethyl polyphenylene sulfide composite material in the preparation of an anti-corrosion material.
[0021] Preferably, the modified graphene oxide / polyvinylidene fluoride / carboxymethyl polyphenylene sulfide composite material is used in the preparation of a metal anti-corrosion coating.
[0022] Ultrasonic dispersion of the composite material in ethanol as a coating and spraying it on the metal surface can achieve the purpose of inhibiting or delaying the decomposition of the metal and causing its corrosion. In addition, the composite material coating formed on the metal surface also has certain salt spray resistance, acid and alkali resistance, and water repellency and antifouling properties, and has broad application prospects in daily life and complex marine environments.
[0023] Therefore, the preparation and application of a modified graphene oxide / polyvinylidene fluoride / carboxymethyl polyphenylene sulfide composite material using the above structure in the present invention has the following beneficial effects:
[0024] (1) Graphene oxide is a graphene derivative with a unique structure and has certain anti-corrosion properties. However, it has many functional groups, such as epoxide, carboxyl and hydroxyl. These functional groups provide active centers, but also weaken its barrier effect as a coating material due to its hydrophilicity. The present invention modifies graphene oxide by octadecylamine. Octadecylamine has a long carbon chain, which makes it highly hydrophobic and has a low thermal conductivity. It can effectively reduce pore wetting, temperature polarization and thermal diffusion across the membrane. This makes the synthesized GO-ODA have a higher specific surface area through the increase of interlayer spacing, and has a higher compatibility with polymers, so that the coating has a better water repellent effect and higher corrosion resistance.
[0025] There is a strong interface interaction between the GO-ODA and PVDF prepared by the present invention. When the two are co-doped, the high temperature resistance of PVDF is improved and the surface morphology, wettability, hydrophobicity, thermal stability and other aspects of the composite coating can be greatly improved.
[0026] Among them, PVDF has high temperature resistance, and its doping as a film-forming agent can improve the disadvantage of unstable high-temperature curing when PPS is used as a coating material.
[0027] (2) Carboxylated polyphenylene sulfide has good rheological properties at high temperatures. Modified graphene oxide and polyvinylidene fluoride are wrapped on the surface of carboxylated polyphenylene sulfide, making its surface more compact. At the same time, the modified graphene oxide doped in it can extend the corrosion path of the corrosive medium, thereby enhancing the anti-corrosion performance of the composite coating. Among them, the addition of polyvinylidene fluoride can change the surface structure of GO-ODA, forming an extra layer of barrier, which can effectively isolate water molecules or delay the contact of corrosion factors with the metal surface, greatly improving the anti-corrosion performance of the coating, while also improving the mechanical properties of the coating.
[0028] (3) Due to the simple preparation method, it is ultrasonically dispersed in ethanol as a coating and sprayed onto the metal surface. The coating can exist stably in the high-humidity and high-salinity marine environment and can play a role in protecting the metal surface. It has broad application prospects in anti-corrosion and anti-fouling environments.
[0029] The technical solution of the present invention is further described in detail below through the accompanying drawings and embodiments. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] Figure 1 The infrared spectra of polyphenylene sulfide, carboxylated polyphenylene sulfide, graphene oxide, octadecylamine and composite material GO-ODA;
[0031] Figure 2 SEM images of carboxylated polyphenylene sulfide, GO, GO-ODA and composite coatings;
[0032] Figure 3 Potentiodynamic polarization curves of GO-ODA / PVDF / PPS coatings with different ratios and the control groups of PPS, PVDF / PPS, GO-ODA / PPS, GO-ODA / PVDF and GO / PVDF / PPS coatings. DETAILED DESCRIPTION
[0033] The present invention will be further described below. It should be noted that this embodiment is based on the technical solution and provides a detailed implementation method and a specific operation process, but the present invention is not limited to this embodiment. Example 1
[0034] A method for preparing a modified graphene oxide / polyvinylidene fluoride / carboxymethyl polyphenylene sulfide composite material comprises the following steps:
[0035] (1) Preparation of carboxylated polyphenylene sulfide: 86.7 g of anhydrous sodium sulfide was weighed and added to 250 mL of N-dimethylpyrrolidone. Nitrogen was continuously introduced to protect the oxygen (nitrogen flow rate was maintained at 10 mL / min). The mixture was reacted at 160°C for 1.5 h to obtain a green anhydrous sodium sulfide solution. After cooling, the solution was poured into a reactor. 0.2 g of catalyst isopropyl titanate was added to the reactor and mixed. Sodium hydroxide was added to adjust the pH of the solution to 12 at room temperature with stirring (stirring speed was 40 r / min). 60.13 g of p-dichlorobenzene and 5.5 g of 2,5-dichlorobenzoic acid were added at 70°C with stirring. Nitrogen was continuously introduced (nitrogen introduction rate was 10 mL / min) with stirring (stirring speed was 1000 r / min). ) to replace the air in the reactor, and then react at 270°C for 2 hours. At this time, the solution is black. It is repeatedly washed with deionized water and ethanol, hot filtered at 50°C, and freeze-dried to obtain carboxylated polyphenylene sulfide, recorded as PPS-COOH.
[0036] (2) Preparation of modified graphene oxide: First, 0.1 g of expanded graphite was dispersed evenly in 100 mL of DMF solution, and ultrasonically exfoliated for 24 h. The obtained product was filtered, washed, and dried to obtain liquid-phase ultrasonically exfoliated graphite flakes. 1 g of the product was added to 120 mL of 0°C mixed acid (90 mL of concentrated sulfuric acid and 30 mL of concentrated phosphoric acid were mixed in an ice-water bath), stirred while maintaining the ice-water bath temperature, and 9 g of potassium permanganate was slowly added. After the reaction was completed, stirring was continued at 50°C for 12 h. After the reaction was completed, 200 mL of ice water and 5 mL of 30% hydrogen peroxide solution were added. It was observed that the color of the solution gradually changed from purple-red to golden yellow. The solution was separated, filtered, washed, and dried to obtain graphene oxide.
[0037] To functionalize graphene oxide, 50 mg of graphene oxide and 200 mg of octadecylamine were first mixed in 50 mL of ethanol and ultrasonically treated for 2 hours. The mixture was then centrifuged at 6000 rpm and washed with ethanol to remove excess octadecylamine. The modified graphene oxide obtained was heated at 130°C in a vacuum for 3 hours to obtain modified graphene oxide, which was recorded as GO-ODA.
[0038] (3) Preparation of modified graphene oxide / polyvinylidene fluoride / carboxylated polyphenylene sulfide composite material: 0.006 g GO-ODA, 0.018 g PVDF, and 0.3 g carboxylated polyphenylene sulfide were added to a round-bottom flask, and 20 mL of solvent ethanol was added. The mixture was dispersed evenly by ultrasonication for 2 h. The mixture was filtered, washed, and freeze-dried at -50 to -60 °C for 12 to 24 h to obtain a modified graphene oxide / polyvinylidene fluoride / carboxylated polyphenylene sulfide composite material.
[0039] (4) Anti-corrosion performance test
[0040] The composite coating was applied according to GB / T 1727-1992 "General Preparation Method for Coatings". The specific method was to disperse the composite material in ethanol at room temperature, and then ultrasonicate to obtain an anticorrosive coating; spray the anticorrosive coating on a clean and dry tinplate with a size of 20×50×1 mm, and cure it in a muffle furnace at 320°C for 3 h, and then conduct an anticorrosive test. Figure 3 As shown, the corrosion potential E c =-256mV, corrosion current I c =7.920×10 -8 A / cm 2 . Example 2
[0041] A method for preparing a modified graphene oxide / polyvinylidene fluoride / carboxymethyl polyphenylene sulfide composite material comprises the following steps:
[0042] (1) Preparation of carboxylated polyphenylene sulfide: Same as Example 1.
[0043] (2) Preparation of modified graphene oxide: same as Example 1.
[0044] (3) Preparation of modified graphene oxide / polyvinylidene fluoride / carboxylated polyphenylene sulfide composite material: 0.009 g GO-ODA, 0.015 g PVDF, and 0.3 g carboxylated polyphenylene sulfide were added to a round-bottom flask, and 20 mL of solvent ethanol was added. The mixture was dispersed evenly by ultrasonic treatment for 2 h. The mixture was filtered, washed, and freeze-dried at -50 to -60 °C for 12 to 24 h to obtain a modified graphene oxide / polyvinylidene fluoride / carboxylated polyphenylene sulfide composite material.
[0045] (4) Anticorrosion performance test: The specific operation is the same as in Example 1; the anticorrosion performance test is as follows Figure 3 As shown, the corrosion potential E c =-115mV, corrosion current I c =9.490×10 -9 A / cm 2 . Example 3
[0046] A method for preparing a modified graphene oxide / polyvinylidene fluoride / carboxymethyl polyphenylene sulfide composite material comprises the following steps:
[0047] (1) Preparation of carboxylated polyphenylene sulfide: Same as Example 1.
[0048] (2) Preparation of modified graphene oxide: same as Example 1.
[0049] (3) Preparation of modified graphene oxide / polyvinylidene fluoride / carboxylated polyphenylene sulfide composite material: 0.012 g GO-ODA, 0.012 g PVDF, and 0.3 g carboxylated polyphenylene sulfide were added into a round-bottom flask, and 20 mL of solvent ethanol was added. The mixture was dispersed evenly by ultrasonic treatment for 2 h. The mixture was filtered, washed, and freeze-dried at -50 to -60 °C for 12 to 24 h to obtain a modified graphene oxide / polyvinylidene fluoride / carboxylated polyphenylene sulfide composite material.
[0050] (4) Anticorrosion performance test: The specific operation is the same as in Example 1; the anticorrosion performance test is as follows Figure 3 As shown, the corrosion potential E c =-342mV, corrosion current I c =3.430×10 -8 A / cm 2 . Example 4
[0051] A method for preparing a modified graphene oxide / polyvinylidene fluoride / carboxymethyl polyphenylene sulfide composite material comprises the following steps:
[0052] (1) Preparation of carboxylated polyphenylene sulfide: Same as Example 1.
[0053] (2) Preparation of modified graphene oxide: same as Example 1.
[0054] (3) Preparation of modified graphene oxide / polyvinylidene fluoride / carboxylated polyphenylene sulfide composite material: 0.015 g GO-ODA, 0.009 g PVDF, and 0.3 g carboxylated polyphenylene sulfide were added into a round-bottom flask, and 20 mL of solvent ethanol was added. The mixture was dispersed evenly by ultrasonic treatment for 2 h. The mixture was filtered, washed, and freeze-dried at -50 to -60 °C for 12 to 24 h to obtain a modified graphene oxide / polyvinylidene fluoride / carboxylated polyphenylene sulfide composite material.
[0055] (4) Anticorrosion performance test: The specific operation is the same as in Example 1; the anticorrosion performance test is as follows Figure 3 As shown, the corrosion potential E c =-232mV, corrosion current I c =1.248×10 -8 A / cm 2 . Example 5
[0056] A method for preparing a modified graphene oxide / polyvinylidene fluoride / carboxymethyl polyphenylene sulfide composite material comprises the following steps:
[0057] (1) Preparation of carboxylated polyphenylene sulfide: Same as Example 1.
[0058] (2) Preparation of modified graphene oxide: same as Example 1.
[0059] (3) Preparation of modified graphene oxide / polyvinylidene fluoride / carboxylated polyphenylene sulfide composite material: 0.018 g GO-ODA, 0.006 g PVDF, and 0.3 g carboxylated polyphenylene sulfide were added into a round-bottom flask, and 20 mL of solvent ethanol was added. The mixture was dispersed evenly by ultrasonic treatment for 2 h. The mixture was filtered, washed, and freeze-dried at -50 to -60 °C for 12 to 24 h to obtain a modified graphene oxide / polyvinylidene fluoride / carboxylated polyphenylene sulfide composite material.
[0060] (4) Anticorrosion performance test: The specific operation is the same as in Example 1; the anticorrosion performance test is as follows Figure 3 As shown, the corrosion potential E c =-335mV, corrosion current I c =1.166×10 -7 A / cm 2 .
[0061] Comparative Example 1
[0062] A method for preparing a graphene oxide / polyvinylidene fluoride / carboxymethyl polyphenylene sulfide composite material comprises the following steps:
[0063] (1) Preparation of carboxylated polyphenylene sulfide: Same as Example 1.
[0064] (2) Preparation of graphene oxide: same as in Example 1.
[0065] (3) Preparation of graphene oxide / polyvinylidene fluoride / carboxylated polyphenylene sulfide composite material: 0.009 g GO, 0.015 g PVDF, and 0.3 g carboxylated polyphenylene sulfide were added to a round-bottom flask, and 20 mL of solvent ethanol was added. The mixture was dispersed evenly by ultrasonication for 2 h. The mixture was filtered, washed, and freeze-dried at -50 to -60 °C for 12 to 24 h to obtain a graphene oxide / polyvinylidene fluoride / carboxylated polyphenylene sulfide composite material.
[0066] (4) Anticorrosion performance test: The specific operation is the same as in Example 1; the anticorrosion performance test is as follows Figure 3 As shown, the corrosion potential E c =-252mV, corrosion current I c =3.429×10 -8 A / cm 2 .
[0067] Comparative Example 2
[0068] A method for preparing a polyvinylidene fluoride / carboxymethyl polyphenylene sulfide composite material comprises the following steps:
[0069] (1) Preparation of carboxylated polyphenylene sulfide: Same as Example 1.
[0070] (2) Preparation of polyvinylidene fluoride / carboxylated polyphenylene sulfide composite material: 0.015 g PVDF and 0.3 g carboxylated polyphenylene sulfide were added to a round-bottom flask, and 20 mL of solvent ethanol was added. The mixture was dispersed evenly by ultrasonic treatment for 2 h, filtered, washed, and freeze-dried at -50 to -60 °C for 12 to 24 h to obtain a polyvinylidene fluoride / carboxylated polyphenylene sulfide composite material.
[0071] (3) Anticorrosion performance test: The specific operation is the same as in Example 1; the anticorrosion performance test is as follows Figure 3 As shown, the corrosion potential E c =-359mV, corrosion current I c =4.677×10 -8 A / cm 2 .
[0072] Comparative Example 3
[0073] A method for preparing a modified graphene oxide / carboxymethyl polyphenylene sulfide composite material comprises the following steps:
[0074] (1) Preparation of carboxylated polyphenylene sulfide: Same as Example 1.
[0075] (2) Preparation of modified graphene oxide: same as Example 1.
[0076] (3) Preparation of modified graphene oxide / carboxylated polyphenylene sulfide composite materials: 0.009 g GO-ODA and 0.3 g carboxylated polyphenylene sulfide were added to a round-bottom flask, and 20 mL of solvent ethanol was added. The mixture was dispersed evenly by ultrasonic treatment for 2 h. The mixture was filtered, washed, and freeze-dried at -50 to -60 °C for 12 to 24 h to obtain a modified graphene oxide / carboxylated polyphenylene sulfide composite material.
[0077] (4) Anticorrosion performance test: The specific operation is the same as in Example 1; the anticorrosion performance test is as follows Figure 3 As shown, the corrosion potential E c =-145mV, corrosion current I c =1.957×10 -7 A / cm 2 .
[0078] Comparative Example 4
[0079] A method for preparing a modified graphene oxide / polyvinylidene fluoride composite material comprises the following steps:
[0080] (1) Preparation of modified graphene oxide: same as in Example 1.
[0081] (2) Preparation of modified graphene oxide / polyvinylidene fluoride composite material: 0.009 g GO-ODA and 0.3 g PVDF were added to a round-bottom flask, and 20 mL of solvent ethanol was added. The mixture was dispersed evenly by ultrasonic treatment for 2 h. The mixture was filtered, washed, and freeze-dried at -50 to -60 °C for 12 to 24 h to obtain a modified graphene oxide / polyvinylidene fluoride composite material.
[0082] (4) Anticorrosion performance test: The specific operation is the same as in Example 1; the anticorrosion performance test is as follows Figure 3 As shown, the corrosion potential E c =-164mV, corrosion current I c =4.163×10 -7 A / cm 2 .
[0083] Comparative Example 5
[0084] A method for preparing a modified graphene oxide / polyvinylidene fluoride / carboxymethyl polyphenylene sulfide composite material comprises the following steps:
[0085] (1) Preparation of carboxylated polyphenylene sulfide: Same as Example 1.
[0086] (2) Preparation of modified graphene oxide: First, 0.1 g of expanded graphite was dispersed evenly in 100 mL of DMF solution, and ultrasonically exfoliated for 24 h. The obtained product was filtered, washed, and dried to obtain liquid-phase ultrasonically exfoliated graphite flakes. 1 g of the product was added to 120 mL of 0°C mixed acid (90 mL of concentrated sulfuric acid and 30 mL of concentrated phosphoric acid were mixed in an ice-water bath), stirred while maintaining the ice-water bath temperature, and 9 g of potassium permanganate was slowly added. After the reaction was completed, stirring was continued at 50°C for 12 h. After the reaction was completed, 200 mL of ice water and 5 mL of 30% hydrogen peroxide solution were added. It was observed that the color of the solution gradually changed from purple-red to golden yellow. The solution was separated, filtered, washed, and dried to obtain graphene oxide.
[0087] To functionalize graphene oxide, 50 mg of graphene oxide and 200 mg of n-pentylamine were first mixed in 50 mL of ethanol and ultrasonically treated for 2 hours. The mixture was then centrifuged at 6000 rpm and washed with ethanol to remove excess octadecylamine. The modified graphene oxide obtained was heated at 130°C in a vacuum for 3 hours to dry, thereby obtaining modified graphene oxide, which was recorded as GO-AA.
[0088] (3) Preparation of modified graphene oxide / polyvinylidene fluoride / carboxylated polyphenylene sulfide composite material: 0.015 g GO-AA, 0.009 g PVDF, and 0.3 g carboxylated polyphenylene sulfide were added into a round-bottom flask, and 20 mL of solvent ethanol was added. The mixture was dispersed evenly by ultrasonic treatment for 2 h. The mixture was filtered, washed, and freeze-dried at -50 to -60 °C for 12 to 24 h to obtain a modified graphene oxide / polyvinylidene fluoride / carboxylated polyphenylene sulfide composite material.
[0089] (4) Anti-corrosion performance test: The specific operation is the same as in Example 1; the anti-corrosion performance test result is the corrosion current I c =2.159×10 -8 A / cm 2 .
[0090] It can be seen from Comparative Example 5 that when a modifier with a shorter carbon chain (n-pentylamine) is used to react with graphene oxide for modification, the corrosion current can still be reduced to a certain extent compared with the GO / PVDF / PPS composite material prepared in Comparative Example 1 and the PVDF / PPS composite material prepared in Comparative Example 2. However, compared with the use of a modifier with a longer carbon chain (octadecylamine) in Example 2, the corrosion current of Example 2 is less than that of Comparative Example 5. The corrosion resistance of the GO-ODA / PVDF / PPS composite material prepared in Example 2 is better than that of the GO-AA / PVDF / PPS composite material prepared in Comparative Example 5, indicating that the use of a modifier with a longer carbon chain to treat graphene oxide can more easily increase the thickness and roughness of the graphene oxide surface, and also more easily increase its specific surface area, thereby increasing the compatibility with other substances (PVDF and PPS) and improving the density of the composite material. Example 6
[0091] The modified graphene oxide / polyvinylidene fluoride / carboxylated polyphenylene sulfide composite materials prepared in Examples 1-5 were subjected to structural analysis and performance characterization.
[0092] (1) Infrared spectroscopy analysis
[0093] Figure 1 The infrared spectra of polyphenylene sulfide, carboxylated polyphenylene sulfide, graphene oxide, octadecylamine and their composite material GO-ODA are shown in Figure 1. According to the spectra, carboxylated polyphenylene sulfide has a similar structure to pure polyphenylene sulfide. In the spectrum of PPS-COOH, 482 cm -1 and 1093 cm -1 The main absorption peak at 1472 cm is related to the stretching vibration of SS and CS bonds. -1 , 1010 cm -1 and 818 cm -1 They correspond to the stretching vibration of the carbon skeleton of the benzene ring of PPS-COOH.-1 and 1180 cm -1 The strong absorption band observed at 3431 cm -1 The non-sharp peak at is attributed to the stretching vibration of -COOH, indicating that PPS-COOH was successfully prepared.
[0094] Comparing the peak positions of graphene oxide and octadecylamine, it can be seen that in the infrared spectrum of modified graphene oxide (GO-ODA), 3435 cm -1 、1639cm -1 The stretching vibrations of the CH single bond and C=O double bond of the amide group are 2921 cm -1 、2850cm -1 、1462cm -1 、719cm -1 Corresponding to the -CH2 stretching vibration of the octadecyl chain on GO-ODA; appears at 1583 cm -1 The new peak is the stretching vibration of the NH single bond, which confirms the reaction between the GO sheets (epoxy groups) and the amine groups in the ODA molecules, indicating that the modification of graphene oxide is successful. -1 (Carboxyl) and 3334cm in ODA -1 The disappearance of the (primary amine) peak indicates that ODA not only reacts with the epoxy group of GO, but also reacts with the -COOH of GO to form secondary amines, among which the nucleophilic substitution reaction between the epoxy group and the amine is the basic reaction, and hydrogen bonding between GO and the oxygen-containing functional groups of the amine and electrostatic attraction between the carboxyl group of GO and the protonated amine also occur.
[0095] (2) Microstructure analysis
[0096] Figure 2 SEM images of carboxylated polyphenylene sulfide, GO, GO-ODA and composite coating.
[0097] Figure 2 a is the SEM image of PPS-COOH. It can be seen from the figure that it is a bouquet-like structure assembled from clustered sheets, and the bouquet sheets are thin and large in size. This ordered structure has a large specific surface area and can provide abundant hole sites for the subsequent co-doping of nanoparticles.
[0098] Figure 2 b and c are SEM images of graphene oxide and modified graphene oxide, respectively. Figure 2 In b, we can see that GO has a thin tulle-like structure with obvious curling wrinkles in the middle and at the edges. Figure 2c shows that the modified GO-ODA sheet structure is significantly thicker and has more pores on the surface, which causes the GO material surface to lose its original smoothness, increases the surface roughness of the material, and reduces the agglomeration of GO in the polymer matrix due to curling and wrinkling. In addition, it greatly prolongs the corrosion path of the corrosive medium, thereby slowing down the corrosion rate of the composite coating. This is attributed to the grafting of octadecylamine on the GO sheet; octadecylamine has a reactive amino group and a long carbon chain. The amino group is used to react with graphene oxide. The long carbon chain can increase the specific surface area of graphene oxide, thereby increasing the corrosion path. When a modification agent with a shorter carbon chain (such as pentylamine) is used, the specific surface area of the modified graphene oxide will decrease, the corrosion path will become shorter, and the corrosion performance will decrease.
[0099] Figure 2 d and e are pure PPS-COOH coating and composite coating, respectively. Compared with pure PPS-COOH coating, the coating surface of the composite material has a distinct concave-convex structure and a dense surface without obvious holes or cracks, and they are entangled with each other, resulting in a very high specific surface area for the composite coating. This may be due to the phase transfer between the modified GO and PVDF during the high-temperature curing process, which causes the surface of the polyphenylene sulfide resin to be covered by it. It is also attributed to the fact that GO-ODA itself has a lamellar structure with a large specific surface area. When thermal cross-linking occurs during the high-temperature solidification process with polyphenylene sulfide, the two cause a large difference in coating roughness, which is beneficial to improving the shielding properties of the composite coating, thereby improving the anti-corrosion performance of the composite coating.
[0100] Figure 2 f is an enlarged image of the composite coating. It can be clearly seen from the figure that there are many intertwined protruding blocks distributed on the surface of carboxylated polyphenylene sulfide. This may be due to the excellent cross-linking effect of PVDF itself. The mechanical properties of the prepared coating can be improved through the network structure constructed by nanoparticles, proving that the GO-ODA / PVDF / PPS composite material and coating were successfully prepared. Example 7
[0101] The impedance performance of the composite coatings prepared in Examples 1-5 and Comparative Examples 1-4 was tested.
[0102] The composite coating was applied in accordance with GB / T 1727-1992 "General Preparation Method for Coatings". The specific method was to disperse the composite material in ethanol at room temperature, and then ultrasonicate to obtain an anti-corrosion coating; the anti-corrosion coating was sprayed on a clean and dry tinplate with a size of 20×50×1 mm, and cured at 320°C in a tube furnace for 3 h to obtain a modified graphene oxide / polyvinylidene fluoride / carboxylated polyphenylene sulfide coating, which was then subjected to an anti-corrosion test.
[0103] Figure 3The potentiodynamic polarization curves of modified graphene oxide and polyvinylidene fluoride composite coatings with different ratios are shown. The test solution is 3.5wt% NaCl solution, and the test items are: polarization curve, corrosion potential, and corrosion current. Figure 3 The data analysis results are as follows: when there is no modified graphene oxide and polyvinylidene fluoride doping, the corrosion potential E of pure PPS-COOH is c =-387mV, corrosion current I c =1.44×10 -7 A / cm 2 The high corrosion current value indicates that the corrosion resistance of PPS-COOH is poor. When the doping ratio of modified graphene oxide to polyvinylidene fluoride is 2:6, the corrosion potential E c =-256mV, corrosion current I c =7.920×10 -8 A / cm 2 , the corrosion current becomes lower, and the anti-corrosion performance of the composite coating is improved. When the doping ratio of modified graphene oxide to polyvinylidene fluoride is 3:5, the corrosion potential E c =-115mV, corrosion current I c =9.490×10 -9 A / cm 2 , at this time, the coating has the lowest corrosion potential and corrosion current. When the amount of modified graphene oxide continues to increase, when the doping amount of modified graphene oxide and polyvinylidene fluoride is 4:4, the corrosion potential E c =-342mV, corrosion current I c =3.430×10 -8 A / cm 2 When the doping ratio of modified graphene oxide to polyvinylidene fluoride is 5:3, the corrosion potential E c =-232mV, corrosion current I c =1.248×10 -8 A / cm 2 , the corrosion current is low, indicating that the appropriate addition of GO-ODA and PVDF can significantly improve the corrosion resistance of the GO-ODA / PVDF / PPS-COOH composite coating. When the doping ratio of modified graphene oxide and polyvinylidene fluoride is 6:2, the corrosion potential E c =-335mV, corrosion current I c =1.166×10 -7 A / cm 2, indicating that continuing to increase the doping amount of nano-graphene oxide causes the nanoparticles to agglomerate, resulting in a decrease in the anti-corrosion performance of the coating. However, for pure PPS-COOH, when GO-ODA and PVDF are added, the anti-corrosion performance is improved compared with pure PPS-COOH.
[0104] In summary, it is shown that when the doping amount of modified graphene oxide and polyvinylidene fluoride is 3:5, the composite coating has the best anti-corrosion performance. The test solution of the present invention is a 3.5wt% NaCl solution. In this high-salt and high-humidity test environment, the present invention can significantly reduce the corrosion current by adding modified graphene oxide and polyvinylidene fluoride to pure carboxylated polyphenylene sulfide, and the corrosion resistance of the composite material is improved. The test solution in the present invention is relatively close to the marine environment, so the composite material prepared by the present invention can be used in the marine environment to prevent and control the corrosion of metal surfaces, such as the metal surface of ships.
[0105] In Comparative Example 1, graphene oxide is directly used to prepare the composite material. Figure 3 It can be seen that the corrosion current of the composite material prepared in Comparative Example 1 is increased compared with that in Example 2, indicating that directly using graphene oxide to prepare the composite material will reduce its corrosion resistance. There are two reasons for the reduction in corrosion resistance. The first is that the surface of graphene oxide has active groups, which makes it hydrophilic. The hydrophilicity will weaken the barrier effect of the coating material. The second is that the surface of graphene oxide is relatively smooth, the specific surface area is small, and the interface interaction with PVDF is weakened. Example 2 Adding octadecylamine to modify graphene oxide not only converts graphene oxide into hydrophobicity, but also uses the carbon chain of octadecylamine to construct a GO-ODA composite material with a large specific surface area. The GO-ODA composite material subsequently produces a strong interface interaction with PVDF, which jointly improves the morphology of the surface of carboxylated polyphenylene sulfide and increases the corrosion resistance. The longer the carbon chain of the added modification reagent (octadecylamine), the more the amino groups in the octadecylamine react with the active groups on the surface of graphene oxide, which can increase the surface roughness and sheet thickness of graphene oxide and prevent graphene oxide from agglomerating.
[0106] In Comparative Example 2, no modified graphene oxide was added, and a PVDF / PPS-COOH composite material was directly formed. Compared with the corrosion currents of Example 2 and Comparative Example 1, the corrosion current of Comparative Example 2 was further increased, indicating that after no modified graphene was added to Comparative Example 2, the corrosion resistance of PPS-COOH could only be changed by PVDF, and the improvement effect of this method was limited.
[0107] Comparative Examples 3 and 4 do not add PVDF and PPS-COOH, respectively, and the corrosion currents of both are greatly increased, indicating that PVDF and PPS-COOH must be present at the same time in the present invention, and PVDF, as a film-forming agent, improves the disadvantage of unstable high-temperature curing of PPS. Comparative Examples 1-4 further illustrate that the modified graphene oxide, PVDF, and PPS-COOH in the present invention must be present at the same time to maximize the corrosion resistance of pure PPS.
[0108] Therefore, the present invention adopts the preparation and application of a modified graphene oxide / polyvinylidene fluoride / carboxymethyl polyphenylene sulfide composite material of the above structure, carboxylated polyphenylene sulfide has good rheological properties at high temperature, modified graphene oxide and polyvinylidene fluoride are wrapped on the surface of carboxylated polyphenylene sulfide to make its surface more compact, and the modified graphene oxide doped therein can extend the corrosion path of the corrosive medium, thereby enhancing the anti-corrosion performance of the composite coating; wherein the addition of polyvinylidene fluoride can change the surface structure of GO-ODA, forming an extra layer of barrier, which can effectively isolate water molecules or delay the contact of corrosion factors with the metal surface, greatly improving the anti-corrosion performance of the coating, and improving the mechanical properties of the coating; the composite material is ultrasonically dispersed in ethanol as a coating, and sprayed onto the metal surface, the coating can stably exist in a high-humidity and high-salinity marine environment, can play a role in protecting the metal surface, and has broad application prospects in anti-corrosion and anti-fouling environments.
[0109] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that they can still modify or replace the technical solution of the present invention with equivalents, and these modifications or equivalent replacements cannot cause the modified technical solution to deviate from the spirit and scope of the technical solution of the present invention.
Claims
1. A method for preparing a modified graphene oxide / polyvinylidene fluoride / carboxymethyl polyphenylene sulfide composite material, characterized in that: The following steps are involved: (1) Preparation of modified graphene oxide Using graphene oxide and octadecylamine as raw materials and ethanol as solvent, the modified graphene oxide is obtained by centrifugation, washing and vacuum drying after ultrasonic treatment; (2) Preparation of carboxylated polyphenylene sulfide: using anhydrous sodium sulfide, p-dichlorobenzene and 2,5-dichlorobenzoic acid as raw materials, N-methylpyrrolidone as solvent, isopropyl titanate as catalyst, nitrogen as protective gas, reacting at 260-280° C. for 1.5-2.5 h in an alkaline environment, washing, filtering and drying to obtain carboxylated polyphenylene sulfide; (3) Preparation of modified graphene oxide / polyvinylidene fluoride / carboxylated polyphenylene sulfide composites Modified graphene oxide, polyvinylidene fluoride and carboxylated polyphenylene sulfide are evenly dispersed in ethanol by ultrasonic dispersion, the amount of modified graphene oxide added is 2% to 6% of the mass of carboxylated polyphenylene sulfide, the mass ratio of modified graphene oxide to polyvinylidene fluoride is 2:6 to 6:2, filtered, washed and freeze-dried to obtain a modified graphene oxide / polyvinylidene fluoride / carboxylated polyphenylene sulfide composite material.
2. The method for preparing a modified graphene oxide / polyvinylidene fluoride / carboxymethyl polyphenylene sulfide composite material according to claim 1, characterized in that: The preparation process of graphene oxide in step (1) is as follows: first, take expanded graphite and disperse it evenly in DMF solvent, ultrasonically peel it for 24 hours, filter, wash and dry the obtained product to obtain liquid-phase ultrasonically peeled graphite flakes, take 1g of it and add it to 120mL of 0°C mixed acid, maintain the temperature of ice water bath and stir, and slowly add potassium permanganate at the same time, stir and react at 50°C for 12 hours, after the reaction is completed, add 200mL of ice water and 5mL of hydrogen peroxide solution, observe that the color of the solution gradually changes from purple-red to golden yellow, separate, filter, wash and dry the solution to obtain graphene oxide.
3. The method for preparing a modified graphene oxide / polyvinylidene fluoride / carboxymethyl polyphenylene sulfide composite material according to claim 2, characterized in that: The volume mass ratio of DMF to expanded graphite is 1L / g; the mixed acid includes a concentrated sulfuric acid solution and a concentrated phosphoric acid solution in a mass ratio of 3:1, the volume mass of the concentrated sulfuric acid solution is 50mL / g, and the volume mass of the concentrated phosphoric acid solution is 30mL / g; the mass ratio of graphite flakes to potassium permanganate is 1:9; and the mass concentration of the H2O2 solution is 30%.
4. The method for preparing a modified graphene oxide / polyvinylidene fluoride / carboxymethyl polyphenylene sulfide composite material according to claim 1, characterized in that: In step (1), the mass ratio of graphene oxide to octadecylamine is 1:4; freeze drying is performed at -60 to -70°C for 12 to 13 hours, and centrifugation is performed at a speed of 6000 rpm; vacuum drying is performed at 110 to 130°C for 3 to 5 hours.
5. The method for preparing a modified graphene oxide / polyvinylidene fluoride / carboxymethyl polyphenylene sulfide composite material according to claim 1, characterized in that: In step (2), the mass ratio of 2,5-dichlorobenzoic acid to anhydrous sodium sulfide is 1:15-1:16, the mass ratio of 2,5-dichlorobenzoic acid to p-dichlorobenzene is 1:10-1:12, and the mass ratio of 2,5-dichlorobenzoic acid to isopropyl titanate is 25:1-30:
1.
6. The method for preparing a modified graphene oxide / polyvinylidene fluoride / carboxymethyl polyphenylene sulfide composite material according to claim 1, characterized in that: In step (3), freeze drying is performed at -50 to -60°C for 12 to 24 hours.
7. Application of the modified graphene oxide / polyvinylidene fluoride / carboxymethyl polyphenylene sulfide composite material obtained by the preparation method according to any one of claims 1 to 6, characterized in that: Application of modified graphene oxide / polyvinylidene fluoride / carboxymethyl polyphenylene sulfide composite materials in the preparation of anti-corrosion materials.
8. The use of the modified graphene oxide / polyvinylidene fluoride / carboxymethyl polyphenylene sulfide composite material according to claim 7, characterized in that: Application of modified graphene oxide / polyvinylidene fluoride / carboxymethyl polyphenylene sulfide composite materials in the preparation of metal anti-corrosion coatings.
Citation Information
Cited By
A preparation method of high temperature resistant and high thermal conductivity PPS composite material
CN119192845B