A high-conductive phosphorus copper alloy material and preparation method thereof
By converting red phosphorus into black phosphorus and combining with graphene oxide, and alloying with copper, magnesium and cerium, the problem of degradation of mechanical properties and corrosion resistance when the conductivity of phosphorus copper alloy materials is improved, and high conductivity is achieved. The coordinated improvement of strength and corrosion resistance is adapted to the needs of modern industrial.
Patent Information
- Application Number
- CN202310368436.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-10
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2043-04-10
AI Technical Summary
While improving the conductivity, existing phosphorus copper alloy materials are difficult to maintain good mechanical properties and corrosion resistance, resulting in limited application range.
Black phosphorus material is prepared by pretreating and catalytic conversion of red phosphorus, combined with graphene oxide to form a phosphorus/graphene composite material, and melt casting with pure copper, magnesium, and cerium, and heat extrusion, drawing and brightening Annealing to prepare a highly conductive phosphorus copper alloy material.
It significantly improves the electrical conductivity and mechanical properties of phosphorus copper alloy materials, ensures that toughness and corrosion resistance are not significantly affected, extends service life, and meets modern industrial needs.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of alloy materials, in particular to a highly conductive phosphorus copper alloy material and a preparation method thereof. Background Art
[0002] At present, phosphor copper alloy is mainly used in printed circuit boards, phosphor copper anodes for electroforming and electroplating, copper strips for electrical equipment contacts and connectors, and is widely used in industries such as motors, central air conditioners, and refrigerators. With the rapid development of modern industry, the performance of the original phosphor copper alloy has been difficult to meet the existing needs. In the current application, phosphor copper alloy is required to have not only better electrical conductivity, but also good mechanical properties and corrosion resistance, so as to enhance the service life and expand the application field.
[0003] In the prior art, better electrical conductivity is usually obtained by increasing the content of red phosphorus. However, there are certain limitations on the improvement of the electrical conductivity of phosphor-copper alloy materials by red phosphorus. As the phosphorus content increases, the toughness and corrosion resistance of the phosphor-copper alloy will be significantly reduced. On the other hand, it will also reduce the mechanical properties of the phosphor-copper alloy, greatly limiting its scope of application.
[0004] In summary, in view of the defects of the prior art, the present invention is committed to solving the problem of increasing the phosphorus content within a suitable range, thereby improving the electrical conductivity of the phosphorus-copper alloy material while limiting its impact on the mechanical properties, toughness and corrosion resistance of the phosphorus-copper alloy material. Summary of the invention
[0005] The object of the present invention is to provide a highly conductive phosphorus copper alloy material and a preparation method thereof, so as to solve the problems raised in the above background technology.
[0006] In order to solve the above technical problems, the present invention provides the following technical solutions:
[0007] A highly conductive phosphorus copper alloy material and a preparation method thereof, comprising the following steps:
[0008] S1: pre-treating and purifying red phosphorus particles to obtain pre-treated red phosphorus;
[0009] S2: catalytically converting, purifying and drying the pretreated red phosphorus to obtain a black phosphorus material, wherein the content of black phosphorus in the black phosphorus material is ≥90%;
[0010] S3: Combining black phosphorus material with graphene oxide to make phosphorus / graphene composite material;
[0011] S4: The phosphorus / graphene composite material is melt-casted with pure copper, magnesium and cerium metals, and then melted, cast, hot extruded, drawn and bright annealed in sequence to obtain a phosphorus-copper alloy material.
[0012] The element composition of the phosphorus copper alloy material is as follows by weight percentage: 84% to 93.9% copper, 6% to 16% phosphorus / graphene composite material (the ratio of phosphorus to graphene is 20:1), 0.05% to 0.1% magnesium, and 0.01% to 0.03% cerium.
[0013] Furthermore, the S1 red phosphorus particles (purity of 77%) are placed in a heating furnace, heated to 250-380°C at a heating rate of 3-8°C / min under a protective atmosphere, maintained for 2-3 hours, and allowed to cool naturally to room temperature; the heat-treated red phosphorus is then ball-milled with a planetary grinder at a rate of 60-300 rpm for 5-30 minutes until it is ground into powder, and placed through a 100-1000 mesh sieve for manual sieving to obtain pretreated red phosphorus.
[0014] The pretreated red phosphorus obtained in the above process was tested for purity, and its purity was ≥99.99%.
[0015] The above-mentioned pretreatment of red phosphorus particles can remove moisture from the raw materials and sublimate the phosphorus pentoxide therein. At the same time, the mixed white phosphorus can be converted into red phosphorus under high temperature conditions to improve the purity of red phosphorus. Finally, the red phosphorus is ground to improve the conversion rate of subsequent black phosphorus preparation.
[0016] Furthermore, the S2 mixes the pretreated red phosphorus with the catalyst gold eutectic foil and tin (the mass ratio of the three is 50:2:1) and seals it in a closed container, evacuates the closed container, injects a protective atmosphere, heats to 600~650℃ at 1.35~1.87℃ / min and maintains for 1~6h, then cools to 500~550℃ at 0.66℃ / min and keeps warm for 1~6h, and finally cools to room temperature at a cooling rate of 1.30~1.50℃ / min to obtain a crude black phosphorus product.
[0017] Furthermore, the crude black phosphorus product obtained in S2 needs to be purified, and the crude black phosphorus product is washed with an alkaline solution, deionized water, and an organic solvent in sequence. After washing, it is dried at 60-100° C. for 0.5-1 h to obtain a black phosphorus material.
[0018] The alkaline solution is 1×10 -3 ~1×10 -2 mol / L calcium hydroxide aqueous solution; the organic solvent includes one or a combination of acetone, chloroform, ether, and carbon tetrachloride.
[0019] The above-mentioned washing of the black phosphorus crude product with an alkaline solution is to remove the red phosphorus impurities therein; the use of deionized water is to clean the alkaline substances; and the organic solvent is to remove Sn and its compounds in the black phosphorus crude product.
[0020] Furthermore, the black phosphorus material obtained in S2 is subjected to a purity test to ensure that its purity is ≥ 90%.
[0021] Furthermore, the preparation method of the phosphorus / graphene composite material in S3 comprises the following specific steps:
[0022] (1) Using isopropanol, graphene oxide and black phosphorus materials are respectively prepared into a solution A of 2 mg / mL to 2.5 mg / mL and a solution B of 20 mg / mL to 25 mg / mL, and the two solutions A and B are mixed evenly, subjected to ultrasonic treatment for 2 to 24 hours, and freeze-dried to obtain a black phosphorus / graphene oxide solid. The black phosphorus / graphene oxide solid is then placed in a protective atmosphere for infrared light pretreatment for 2 to 72 hours to obtain a phosphorus / pre-reduced graphene oxide solid;
[0023] (2) Under a protective atmosphere, the phosphorus / pre-reduced graphene oxide solid is heated in a range of 50 to 150° C. for a heating time of 0.5 h to 3 h to obtain a phosphorus / graphene composite material for use.
[0024] The above-mentioned use of graphene oxide and black phosphorus material for compounding to prepare phosphorus / graphene composite materials, abandoning the previous use of red phosphorus for phosphorus copper alloy material preparation, and using black phosphorus, compared to red phosphorus, black phosphorus has excellent electrical conductivity, and other aspects of performance are more excellent than red phosphorus, using it and copper to make phosphorus copper alloy materials, the performance of the alloy will be more excellent; at the same time, graphene and black phosphorus are introduced, because graphene has good electrical conductivity, thermal conductivity and toughness, while improving the electrical conductivity of phosphorus copper alloy materials, it also solves the brittleness problem caused by excessive phosphorus content, and can also help the alloy material to dissipate heat better, reducing the influence of excessive temperature during use, resulting in increased resistance, and the decrease in the electrical conductivity of the material. In addition, due to the purity of black phosphorus material, it is inevitable that a small amount of nano red phosphorus is doped therein, and graphene can form a three-dimensional layered thermal conductive system composed of flakes and granules with nano red phosphorus, forming a red phosphorus / graphene composite material, which indirectly weakens the influence of nano red phosphorus on the poor mechanical properties of phosphorus copper alloy materials, and further improves the thermal conductivity of the material.
[0025] Furthermore, the phosphorus copper alloy material preparation step in S4 is:
[0026] (1) Pure copper, magnesium and rare earth metal cerium are placed in a closed crucible, a protective gas is introduced, and the mixture is heated to 1100°C until the metal is completely melted. Then, the phosphorus / graphene composite material obtained in S3 is added, and the mixture is stirred evenly and then taken out of the furnace and cast into an ingot;
[0027] (2) The ingot is subjected to hot extrusion, drawing, bright annealing in sequence, and finally cooled to obtain a phosphorus copper alloy material.
[0028] The ingot is heated by hot extrusion using an induction heating furnace; and bright annealing uses an atmosphere-protected bright annealing resistance furnace.
[0029] The above preparation of phosphor copper alloy material, melting in a closed crucible can isolate air, avoid mixing with oxygen, resulting in more pores in the product, thereby damaging the mechanical properties and electrical conductivity of the material; subsequent treatment of the material can further improve the material strength and corrosion resistance, and can also obtain a brighter and smoother material; magnesium and rare earth metal cerium are introduced into the alloy, magnesium can increase the strength, toughness and corrosion resistance of the alloy, cerium can significantly improve the oxidation resistance of the alloy, copper alloying effect, reduce the alloy activity, modify the alloy surface, improve the alloy quality, further improve the alloy strength and toughness, and extend the service life of the alloy. In addition, since a small amount of red phosphorus / graphene composite material is doped in the phosphorus / graphene composite material, graphene can form a three-dimensional layered thermal conductive system composed of flakes and granules with nano red phosphorus, forming a red phosphorus / graphene composite material, which indirectly weakens the bad influence of nano red phosphorus on the mechanical properties of phosphor copper alloy materials and further improves the thermal conductivity of the material.
[0030] Compared with the prior art, the beneficial effects achieved by the present invention are:
[0031] The phosphor copper alloy material prepared by the present invention fully improves the defects of strength, toughness and corrosion resistance of the product under the cooperation of graphene, magnesium and rare earth metal cerium. While improving the electrical conductivity of the phosphor copper alloy, it can ensure that the toughness and corrosion resistance of the phosphor copper alloy will not be significantly affected, and at the same time, the thermal conductivity of the material is also improved, and the electrical conductivity of the material is more stable.
[0032] In summary, the product of the present invention has largely solved the defects of high-conductivity phosphor-copper alloy materials in the application of related industries, can better adapt to the needs of modern industry, and can also be more widely used in other industries. DETAILED DESCRIPTION
[0033] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0034] In the following examples, the purity of red phosphorus particles is 77%, Zhengzhou Chemical International Co., Ltd.; the purity of graphene oxide is greater than 99%, single layer, sheet diameter: 0.5~5μm, thickness: 0.8~1.2nm, Yunguan (Shanghai) Biotechnology Co., Ltd.; the purity of pure copper is 99.99%, Wuhan Xinrong New Materials Co., Ltd.; the purity of magnesium is 99.95%, Shandong Yicheng Steel Co., Ltd.; the purity of cerium is 99.99%, Beijing Quanta Ruijin Chemical Co., Ltd.; the purity of Jinxi eutectic foil is 99.99%, 0.1mm (thickness) × 43.88mm (width), Alfa Aesar (China) Chemical Co., Ltd.; the purity of tin is 99%. Shandong Tianming Biotechnology Development Co., Ltd.
[0035] Examples 1 to 3 and Comparative Examples 1 to 6 all use raw materials in the mass percentages shown in the following table. Example
[0036] A highly conductive phosphorus copper alloy material and a preparation method thereof, comprising the following steps:
[0037] S1: pre-treating and purifying red phosphorus particles to obtain pre-treated red phosphorus;
[0038] The red phosphorus particles are placed in a heating furnace, heated to 280°C at a heating rate of 6°C / min under a protective atmosphere, maintained for 2 hours, and allowed to cool naturally to room temperature; the heat-treated red phosphorus is then ball-milled using a planetary grinder at a rate of 100 rpm for 10 minutes until it is ground into powder, and placed through a 425-mesh sieve for manual sieving to obtain pretreated red phosphorus.
[0039] S2: catalytically converting, purifying and drying the pretreated red phosphorus to obtain black phosphorus material;
[0040] The pretreated red phosphorus was mixed evenly with the catalyst gold eutectic foil and tin (the mass ratio of the three was 50:2:1), sealed in a sealed container, evacuated, injected with a protective atmosphere, heated to 600°C at 1.57°C / min and maintained for 3h, then cooled to 550°C at 0.66°C / min and maintained for 3h, and finally cooled to room temperature at a cooling rate of 1.35°C / min to obtain a crude black phosphorus product.
[0041] The crude black phosphorus product obtained in S2 is purified, and the purification steps are as follows:
[0042] (1) Use 1×10 -2 The black phosphorus material was washed twice with a mol / L calcium hydroxide aqueous solution;
[0043] (2) continuing to wash the black phosphorus material washed in (1) with deionized water until the pH value of the deionized water is neutral;
[0044] (3) Wash the black phosphorus material obtained in (2) with acetone until the organic solvent no longer changes color.
[0045] The black phosphorus material obtained in (3) was dried in a vacuum drying oven at 60°C for 1 h.
[0046] The purity of the black phosphorus material after washing and purification was tested and the purity was 95%.
[0047] S3: Combining black phosphorus with graphene to prepare a phosphorus / graphene composite material, comprising the following steps;
[0048] (1) Using isopropanol, graphene oxide and black phosphorus materials were prepared into 2 mg / mL solution A and 20 mg / mL solution B, respectively. Solutions A and B were mixed evenly, and after ultrasonic treatment for 12 hours, freeze-dried to obtain black phosphorus / graphene oxide solid. The solid was placed in a protective atmosphere for infrared light pretreatment for 24 hours to obtain black phosphorus / pre-reduced graphene oxide solid;
[0049] (2) The black phosphorus / pre-reduced graphene oxide solid is heated to 100° C. for 2 h under a protective atmosphere to obtain a phosphorus / graphene composite material for use.
[0050] S4: The phosphorus / graphene composite material and pure copper are processed and prepared, comprising the following steps:
[0051] (1) Pure copper, magnesium and rare earth metal cerium are placed in a closed crucible, a protective gas is introduced, and the mixture is heated to 1100°C until the metal is completely melted. Then, the phosphorus / graphene composite material obtained in S3 is added, and the mixture is stirred evenly and then taken out of the furnace and cast into an ingot;
[0052] (2) The ingot is subjected to hot extrusion, drawing, bright annealing in sequence, and finally cooled to obtain a phosphorus copper alloy material.
[0053] The ingot is heated by hot extrusion using an induction heating furnace; and bright annealing uses an atmosphere-protected bright annealing resistance furnace. Example
[0054] A highly conductive phosphorus copper alloy material and a preparation method thereof, comprising the following steps:
[0055] S1: pre-treating and purifying red phosphorus particles to obtain pre-treated red phosphorus;
[0056] The red phosphorus particles are placed in a heating furnace, heated to 250°C at a heating rate of 3°C / min under a protective atmosphere, maintained for 2 hours, and allowed to cool naturally to room temperature; the heat-treated red phosphorus is then ball-milled using a planetary grinder at a rate of 60 rpm for 5 minutes until it is ground into powder, and placed through a 250-mesh sieve for manual sieving to obtain pretreated red phosphorus.
[0057] S2: catalytically converting, purifying and drying the pretreated red phosphorus to obtain black phosphorus material;
[0058] The pretreated red phosphorus was mixed evenly with the catalyst gold eutectic foil and tin (the mass ratio of the three was 50:2:1), sealed in a sealed container, evacuated, injected with a protective atmosphere, heated to 600°C at 1.35°C / min and maintained for 3h, then cooled to 550°C at 0.66°C / min and kept for 1h, and finally cooled to room temperature at a cooling rate of 1.30°C / min to obtain a crude black phosphorus product.
[0059] The crude black phosphorus product obtained in S2 is purified, and the purification steps are as follows:
[0060] (1) Use 1×10 -3 The black phosphorus material was washed once with a mol / L calcium hydroxide aqueous solution;
[0061] (2) continuing to wash the black phosphorus material washed in (1) with deionized water until the pH value of the deionized water is neutral;
[0062] (3) Wash the black phosphorus material obtained in (2) with acetone until the organic solvent no longer changes color.
[0063] The black phosphorus material obtained in (3) was dried in a vacuum drying oven at 60°C for 0.5 h.
[0064] The purity of the black phosphorus material after washing and purification was tested and the purity was 91%.
[0065] S3: Combining black phosphorus with graphene to prepare a phosphorus / graphene composite material, comprising the following steps;
[0066] (1) Graphene oxide and black phosphorus materials were prepared into 2 mg / mL solution A and 20 mg / mL solution B respectively using isopropanol. Solutions A and B were mixed evenly, and after ultrasonic treatment for 2 h, freeze-dried to obtain black phosphorus / graphene oxide solid. The solid was placed in a protective atmosphere for infrared light pretreatment for 6 h to obtain black phosphorus / pre-reduced graphene oxide solid;
[0067] (2) The black phosphorus / pre-reduced graphene oxide solid is heated to 100° C. under a protective atmosphere for 1 h to obtain a phosphorus / graphene composite material for use.
[0068] S4: The phosphorus / graphene composite material and pure copper are processed and prepared, comprising the following steps:
[0069] (1) Pure copper, magnesium and rare earth metal cerium are placed in a closed crucible, a protective gas is introduced, and the mixture is heated to 1100°C until the metal is completely melted. Then, the phosphorus / graphene composite material obtained in S3 is added, and the mixture is stirred evenly and then taken out of the furnace and cast into an ingot;
[0070] (2) The ingot is subjected to hot extrusion, drawing, bright annealing in sequence, and finally cooled to obtain a phosphorus copper alloy material.
[0071] The ingot is heated by hot extrusion using an induction heating furnace; and bright annealing uses an atmosphere-protected bright annealing resistance furnace. Example
[0072] A highly conductive phosphorus copper alloy material and a preparation method thereof, comprising the following steps:
[0073] S1: pre-treating and purifying red phosphorus particles;
[0074] The red phosphorus particles are placed in a heating furnace, heated to 380°C at a heating rate of 8°C / min under a protective atmosphere, maintained for 3 hours, and allowed to cool naturally to room temperature; the heat-treated red phosphorus is then ball-milled using a planetary grinder at a rate of 300 revolutions / min for 30 minutes until it is ground into powder, and placed through a 1000-mesh sieve for manual sieving to obtain pretreated red phosphorus.
[0075] S2: catalytically converting, purifying and drying the pretreated red phosphorus to obtain black phosphorus material;
[0076] The pretreated red phosphorus was mixed evenly with the catalyst gold eutectic foil and tin (the mass ratio of the three was 50:2:1), sealed in a sealed container, evacuated, injected with a protective atmosphere, heated to 650°C at 1.87°C / min and maintained for 6 hours, then cooled to 550°C at 0.66°C / min and maintained for 6 hours, and finally cooled to room temperature at a cooling rate of 1.50°C / min to obtain a crude black phosphorus product.
[0077] The crude black phosphorus product obtained in S2 is purified, and the purification steps are as follows:
[0078] (1) Use 1×10 -2 The black phosphorus material was washed twice with a mol / L calcium hydroxide aqueous solution;
[0079] (2) continuing to wash the black phosphorus material washed in (1) with deionized water until the pH value of the deionized water is neutral;
[0080] (3) Wash the black phosphorus material obtained in (2) with acetone until the organic solvent no longer changes color.
[0081] The black phosphorus material obtained in (3) was dried in a vacuum drying oven at 100°C for 1 h.
[0082] The purity of the black phosphorus material after washing and purification was tested and the purity was 98%.
[0083] S3: Combining black phosphorus with graphene to prepare a phosphorus / graphene composite material, comprising the following steps;
[0084] (1) Graphene oxide and black phosphorus materials were prepared into 2.5 mg / mL solution A and 25 mg / mL solution B respectively using isopropanol. Solutions A and B were mixed evenly, and after ultrasonic treatment for 24 hours, freeze-dried to obtain black phosphorus / graphene oxide solid. The solid was placed in a protective atmosphere for infrared light pretreatment for 72 hours to obtain black phosphorus / pre-reduced graphene oxide solid;
[0085] (2) The black phosphorus / pre-reduced graphene oxide solid is heated to 150° C. under a protective atmosphere for 3 h to obtain a phosphorus / graphene composite material for use.
[0086] S4: The phosphorus / graphene composite material and pure copper are processed and prepared, comprising the following steps:
[0087] (1) Pure copper, magnesium and rare earth metal cerium are placed in a closed crucible, a protective gas is introduced, and the mixture is heated to 1100°C until the metal is completely melted. Then, the phosphorus / graphene composite material obtained in S3 is added, and the mixture is stirred evenly and then taken out of the furnace and cast into an ingot;
[0088] (2) The ingot is subjected to hot extrusion, drawing, bright annealing in sequence, and finally cooled to obtain a phosphorus copper alloy material.
[0089] The ingot is heated by hot extrusion using an induction heating furnace; and bright annealing uses an atmosphere-protected bright annealing resistance furnace.
[0090] Comparative Example 1:
[0091] No magnesium or rare earth metal cerium was added, and the rest was the same as in Example 1;
[0092] Comparative Example 2:
[0093] Without introducing graphene, the rest is the same as Example 1;
[0094] Comparative Example 3:
[0095] The purified red phosphorus is directly used with pure copper powder for preparation and processing, and the other aspects are the same as those in Example 1;
[0096] Comparative Example 4:
[0097] The purified red phosphorus and uniform alloy powder are used for preparation and processing, and the other aspects are the same as those in Example 1;
[0098] Comparative Example 5:
[0099] The preparation and processing are carried out using black phosphorus material and pure copper powder, and the rest is the same as Example 1;
[0100] Comparative Example 6:
[0101] A red phosphorus / graphene composite material was prepared by using pretreated red phosphorus and graphene oxide, and the rest was the same as in Example 1.
[0102] Performance test: The prepared phosphor copper alloy material was subjected to conductivity test and tensile strength test. Samples of the same size were taken from Examples 1 to 3 and Comparative Examples 1 to 6 for inspection. The conductivity was tested using a D60K digital metal conductivity meter. The sample was polished before testing. The tensile strength was tested using a universal testing machine according to the standard of GB / T 34505-2017. The obtained data are shown below:
[0103]
[0104] From the data of Examples 1 to 3 in the above table, it can be seen that increasing the content of black phosphorus within a certain degree can increase the electrical conductivity and tensile strength of the phosphorus copper alloy, and excessive introduction will lead to a decrease in its performance; from the comparison of the data of Comparative Examples 1 to 6 with Examples 1 to 3, it can be seen that the introduction of black phosphorus, the composite of graphene and phosphorus, and magnesium and cerium all improve the electrical conductivity and tensile strength of the phosphorus copper alloy material to a certain extent. Compared with directly composite red phosphorus with copper, the composite of phosphorus / graphene composite material and copper improves the electrical conductivity and strength significantly.
[0105] Finally, it should be noted that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for preparing a highly conductive phosphorus copper alloy material, characterized in that: The following steps are involved: S1: pre-treating and purifying red phosphorus particles to obtain pre-treated red phosphorus; S2: catalytically converting, purifying and drying the pretreated red phosphorus to obtain a black phosphorus material, wherein the content of black phosphorus in the black phosphorus material is ≥90%; S3: Combining black phosphorus material with graphene oxide to make phosphorus / graphene composite material; S4: The phosphorus / graphene composite material is melt-casted with pure copper, magnesium and cerium metals, and then melted, cast, hot extruded, drawn and bright annealed in sequence to obtain a phosphorus-copper alloy material.
2. The method for preparing a highly conductive phosphorus copper alloy material according to claim 1, characterized in that: In S1, the specific process is: the red phosphorus particles are placed in a heating furnace, and the temperature is increased to 250~380°C at a heating rate of 3~8°C / min under a protective atmosphere, and maintained for 2~3 hours, and then naturally cooled to room temperature, and then the heat-treated red phosphorus is ball-milled with a planetary grinder at a rate of 60~300 rpm for 5~30 minutes, ground into powder, and put into a 100~1000 mesh sieve for manual sieving to obtain pretreated red phosphorus.
3. The method for preparing a highly conductive phosphorus copper alloy material according to claim 1, characterized in that: In S2, the pretreated red phosphorus is mixed evenly with the catalyst gold eutectic foil and tin, and then sealed in a closed container, the closed container is evacuated, and a protective atmosphere is injected and heated to 600~650℃ at 1.35~1.87℃ / min and maintained for 1~6h, then cooled to 500~550℃ at 0.66℃ / min and kept warm for 1~6h, and finally cooled to room temperature at a cooling rate of 1.30~1.50℃ / min to obtain a crude black phosphorus product. Finally, the crude black phosphorus product is washed with an alkaline solution, deionized water, and an organic solvent in sequence. After washing, it is dried at 60~100℃ for 0.5~1h to obtain a black phosphorus material.
4. The method for preparing a highly conductive phosphorus copper alloy material according to claim 3, characterized in that: The mass ratio of the pretreated red phosphorus, gold eutectic foil and tin is 50:2:
1.
5. The method for preparing a highly conductive phosphorus copper alloy material according to claim 3, characterized in that: The alkaline solution is 1×10 -3 ~1×10 -2 mol / L calcium hydroxide aqueous solution.
6. The method for preparing a highly conductive phosphorus copper alloy material according to claim 3, characterized in that: The organic solvent includes one or a combination of acetone, chloroform, ether and carbon tetrachloride.
7. The method for preparing a highly conductive phosphorus copper alloy material according to claim 1, characterized in that: The specific process in S3 is: (1) Using isopropanol, graphene oxide and black phosphorus materials are respectively prepared into a solution A of 2 mg / mL to 2.5 mg / mL and a solution B of 20 mg / mL to 25 mg / mL, and the two solutions A and B are mixed evenly, subjected to ultrasonic treatment for 2 to 24 hours, and freeze-dried to obtain a black phosphorus / graphene oxide solid. The black phosphorus / graphene oxide solid is then placed in a protective atmosphere for infrared light pretreatment for 2 to 72 hours to obtain a black phosphorus / pre-reduced graphene oxide solid; (2) The black phosphorus / pre-reduced graphene oxide solid is heated under a protective atmosphere at a temperature of 50 to 300° C. for a heating time of 0.5 h to 10 h to obtain a phosphorus / graphene composite material for use.
8. The method for preparing a highly conductive phosphorus copper alloy material according to claim 1, characterized in that: The specific process in S4 is: (1) Pure copper, magnesium and rare earth metal cerium are placed in a closed crucible, a protective gas is introduced, and the mixture is heated to 1100°C until the metal is completely melted. Then, the phosphorus / graphene composite material obtained in S3 is added, and the mixture is stirred evenly and then taken out of the furnace and cast into an ingot; (2) The ingot is subjected to hot extrusion, drawing, bright annealing in sequence, and finally cooled to obtain a phosphorus copper alloy material.
9. The phosphor-copper alloy material prepared by the method for preparing a highly conductive phosphor-copper alloy material according to any one of claims 1 to 8, characterized in that: The phosphorus copper alloy material is composed of the following raw materials: by weight percentage: 83.9-93.9% copper, 6-16% phosphorus / graphene composite material, 0.05-0.1% magnesium, and 0.01-0.03% cerium.