A kind of non-ironing skin-friendly polyester-viscose fabric and preparation method thereof

Through the esterification reaction, 3,4-dihydroxyphenylpropionic acid is grafted with polyester fiber and viscose fiber to form a cross-linked network structure, which solves the problem of poor ironing properties of polyester and viscose fabrics and achieves high ironing properties and skin-friendly properties. Fabric preparation avoids the production of formaldehyde and maintains the elasticity and comfort of the fabric.

CN116463852BActive Publication Date: 2024-10-01HANGZHOU CHENHAO TEXTILE FINISHING CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310503032.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-05-06
Publication Date
2024-10-01
Estimated Expiration
2043-05-06

AI Technical Summary

Technical Problem

The existing polyester-viscose fabrics obtained by blending polyester fiber and viscose fiber have poor ironing properties, and the commonly used easy-iron finishing agents contain formaldehyde, which is harmful to human health and the environment. At the same time, the fabric becomes fragile after finishing and the skin-friendly feeling is reduced.

Method used

Grafting 3,4-dihydroxyphenylpropionic acid through an esterification reaction forms a cross-linked network structure with polyester fiber and viscose fiber, inhibiting fiber slippage and deformation, and increasing hygroscopicity and cross-linking through modified polyester fiber. The fabric is interconnected to form a fabric with good iron-free properties and skin-friendly properties.

Benefits of technology

It improves the ironing-free and comfortable properties of polyester-viscose fabrics, avoids the generation of formaldehyde, maintains the fabric's elasticity and skin-friendly feel, and is environmentally friendly.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004214515720000061
    Figure BDA0004214515720000061
  • Figure BDA0004214515720000071
    Figure BDA0004214515720000071
Patent Text Reader

Abstract

The present application discloses a non-ironing skin-friendly polyester-viscose fabric and a preparation method thereof. The non-ironing skin-friendly polyester-viscose fabric is obtained by blending polyester fiber and viscose fiber and finishing. The non-ironing skin-friendly polyester-viscose fabric is grafted with 3,4-dihydroxyphenylpropionic acid through esterification reaction during the finishing process. The polyester fiber is modified and grafted, and the skin-friendliness of the fabric is increased; 3,4-dihydroxyphenylpropionic acid can be cross-linked with the modified grafted polyester fiber and viscose fiber to form a cross-linked network structure, and 3,4-dihydroxyphenylpropionic acid contains benzene rings and short alkyl chains. The cross-linked network structure and the rigid benzene ring structure can effectively inhibit the relative displacement between fiber molecules of the fabric when the fabric is subjected to external force, and the short alkyl chain can drive the cross-linked viscose fiber to recover through internal rotation, thereby increasing the non-ironing property of the fabric.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of polyester-viscose fabrics, and in particular to a wrinkle-free, skin-friendly polyester-viscose fabric and a preparation method thereof. Background Art

[0002] Polyester fabric has good dimensional stability, friction resistance, electrical insulation, and chemical resistance, but poor air permeability and moisture dissipation. Viscose fiber has antistatic properties, good air permeability and humidity regulation functions. Blending polyester fiber with viscose fiber can reduce the cost of wool fabrics without affecting the appearance of wool fabrics. On the other hand, the addition of viscose fiber can improve the strength and fluffiness of the fabric.

[0003] However, the polyester-viscose fabric obtained by blending polyester fiber and viscose fiber has poor ironing resistance. Chemical reagents are usually used to perform ironing-free finishing on the fabric. However, most of the commonly used ironing-free finishing agents contain formaldehyde, which has an impact on human health and the natural environment. At the same time, after ironing-free finishing, the fabric becomes fragile, has poor elasticity, and its skin-friendly feel is significantly reduced. Summary of the Invention

[0004] In order to solve the problem of improving the wrinkle-free property of polyester-viscose fabric while maintaining good skin-friendliness of the fabric, and to be green and environmentally friendly during the wrinkle-free finishing process, the present application provides a wrinkle-free skin-friendly polyester-viscose fabric and a preparation method thereof.

[0005] In a first aspect, the present application provides a wrinkle-free skin-friendly polyester-viscose fabric, which is obtained by blending polyester fiber and viscose fiber and then finishing the blended polyester-viscose fabric. The wrinkle-free skin-friendly polyester-viscose fabric is grafted with 3,4-dihydroxyphenylpropionic acid through an esterification reaction during the finishing process.

[0006] The poor wrinkle-free property of polyester and viscose fibers is mainly due to the fact that when subjected to external force, the fibers bend and deform, slip, and the basic structural units of the fiber macromolecules produce relative displacement. Viscose fibers contain a large number of hydroxyl groups, which form hydrogen bonds at new positions. After the external force is removed, the fiber molecules recover slowly due to the blocking effect of the new hydrogen bonds formed at the new positions. When the external force is too large, the fiber will undergo irreversible deformation.

[0007] By adopting the above technical solution, 3,4-dihydroxyphenylpropionic acid, after a finishing process, acts on polyester-viscose fibers through an esterification reaction. 3,4-dihydroxyphenylpropionic acid contains benzene rings, which have high rigidity and can inhibit the molecular structure of the fiber from slipping when subjected to stress, thereby increasing the wrinkle-free properties of the polyester-viscose fabric. Furthermore, 3,4-dihydroxyphenylpropionic acid contains short -CH2-CH2-alkyl chains, which have good internal rotation recovery properties and can quickly return to their original position after the external force is removed. This internal rotation recovery property also improves the elasticity of the fiber, thereby increasing the comfort and wrinkle-free properties of the fabric.

[0008] In addition, after the carboxyl group in 3,4-dihydroxyphenylpropionic acid reacts and cross-links with the hydroxyl group in viscose fiber, it can inhibit the viscose fiber from forming new hydrogen bonds, and after the external force is removed, the short alkyl chain can drive the viscose fiber to return to its original position, which can enhance the wrinkle-free property of polyester-viscose fabrics.

[0009] Preferably, during the finishing process, the mass ratio of the polyester-viscose fabric, 3,4-dihydroxyphenylpropionic acid and the esterification reaction catalyst is 100:(6-10):(0.04-0.12).

[0010] Preferably, the esterification reaction catalyst includes one or more of thionyl chloride, p-toluenesulfonic acid, sodium acetate, and potassium bisulfate.

[0011] Preferably, the finishing process of the wrinkle-free and skin-friendly polyester-viscose fabric is as follows: polyester fiber and viscose fiber are blended to obtain polyester-viscose fabric; a finishing agent is added to deionized water, and then an esterification reaction catalyst is added, mixed evenly to obtain a finishing agent aqueous solution, and the polyester-viscose fabric is immersed in the finishing agent aqueous solution, the temperature of the finishing agent aqueous solution is adjusted to 35-45°C, and the immersion is 60-80 minutes.

[0012] By employing this technical solution, 3,4-dihydroxyphenylpropionic acid fully diffuses into the molecular structure of polyester-viscose fibers during the finishing and impregnation process. Under the action of an esterification catalyst, it chemically crosslinks with the polyester-viscose fabric, forming a cross-linked network structure. When subjected to external forces, this cross-linked network structure inhibits fiber deformation and slippage, preventing relative displacement of the fiber molecules. Furthermore, after the force is removed, the fiber exhibits excellent recovery, resulting in excellent iron-free properties for the polyester-viscose fabric. This process also eliminates the production of harmful byproducts such as formaldehyde.

[0013] At the same time, 3,4-dihydroxyphenylpropionic acid penetrates between the fiber molecules of polyester-viscose fabrics. The cross-linked network structure formed between the fiber molecules can effectively prevent the fibers from being pulled out from spinning, while inhibiting the twisting and deformation of the fibers after being subjected to external force or friction, which can effectively improve the anti-pilling performance of polyester-viscose fabrics.

[0014] Preferably, the polyester fiber is a modified polyester fiber grafted with a dicarboxy vinyl compound.

[0015] Preferably, the dicarboxy vinyl compound includes one or more of maleic acid, fumaric acid, glutaric acid, and hexadienedioic acid.

[0016] Preferably, the raw materials of the modified polyester fiber include polyester fiber, dicarboxy vinyl compound and initiator in a mass ratio of 100:(15-25):(0.2-0.5).

[0017] By adopting the above technical solution, the dicarboxyl vinyl compound contains hydrophilic groups. After being grafted onto the polyester fiber, the hydrophilic carboxyl groups are attached to the surface of the polyester fiber, changing the polyester fiber from hydrophobic to hydrophilic. This can effectively increase the hygroscopicity of the polyester fiber and improve the comfort and skin-friendliness of the polyester-viscose fabric. At the same time, the carboxyl groups grafted onto the surface of the polyester fiber can cross-link with the hydroxyl groups in 3,4-dihydroxyphenylpropionic acid, facilitating the formation of a cross-linked network structure and effectively inhibiting fiber slippage. In addition, the polyester fiber itself has a short -CH2-CH2-alkyl chain, which can increase the recovery of the system and help increase the wrinkle-free properties of the polyester-viscose fiber.

[0018] Preferably, the modified grafting steps of the modified polyester fiber are as follows: immersing the polyester fiber in a swelling agent for swelling treatment; adding an initiator and a dicarboxylic acid vinyl compound to deionized water and stirring and mixing to obtain a grafting solution; under the protection of an inert gas atmosphere, immersing the swollen polyester fiber in the grafting solution, adjusting the solution temperature to 30-40°C, stirring and reacting for 2-3 hours, and then washing with water to obtain the modified polyester fiber.

[0019] Preferably, the swelling agent includes one or more of acetic acid, acetone, chloroform, and phenol aqueous solutions with a mass fraction of 2%.

[0020] Preferably, the mass ratio of the swelling agent to the polyester fiber is (1.5-2):1.

[0021] Preferably, the initiator includes one or more of hydrogen peroxide, benzoyl peroxide, and azobisisobutyronitrile.

[0022] By adopting the above technical solution, the polyester fiber is first swollen with a swelling agent, the gaps between the fiber molecules become larger, and then in the subsequent grafting process, the dicarboxyl vinyl compound can effectively diffuse into the polyester fiber, increasing the grafting rate and improving the hydrophilicity of the polyester fiber, thereby increasing the skin-friendliness of the polyester-viscose fabric.

[0023] Preferably, the polyester fiber is a polyester fiber with a special-shaped cross-section.

[0024] Preferably, the heterogeneous cross-section polyester fiber includes one of a triangular, pentaf-shaped, flat ribbon-shaped, and cross-shaped cross-section polyester fiber.

[0025] By adopting the above technical solution, on the one hand, the elastic modulus and deformation resistance of the special-shaped cross-section polyester fiber are better than those of ordinary round fibers, and the wrinkle-free property of the polyester-viscose fabric produced is increased; on the other hand, after the special-shaped cross-section polyester fiber is blended with the circular cross-section viscose fiber, a certain gap can be formed inside the fabric, which is conducive to the evaporation of moisture. After the fabric absorbs sweat or other liquids, the sweat or other liquids can evaporate through the gaps, thereby increasing the moisture-wicking property of the fabric, thereby increasing the comfort and skin-friendliness of the polyester-viscose fabric.

[0026] Preferably, the mass ratio of the polyester fiber to the viscose fiber is (63-76):(33-37).

[0027] In a second aspect, the present application provides a method for preparing a wrinkle-free, skin-friendly polyester-viscose fabric, comprising the following steps:

[0028] Finishing and modification: The modified polyester fiber is blended with viscose fiber to obtain polyester-viscose fabric, and the polyester-viscose fabric is subjected to impregnation finishing and esterification reaction to obtain impregnated polyester-viscose fabric;

[0029] Heat setting: Dry the impregnated fabric at 70-80℃ for 15-20 minutes; bake the dried fabric at 115-125℃ for 3-5 minutes to obtain the wrinkle-free and skin-friendly polyester-viscose fabric.

[0030] In summary, this application has the following beneficial effects:

[0031] 1. The wrinkle-free, skin-friendly polyester-viscose fabric of this application is grafted with 3,4-dihydroxyphenylpropionic acid through an esterification reaction during the finishing process. On the one hand, the rigid benzene ring structure contained in 3,4-dihydroxyphenylpropionic acid can inhibit relative displacement of the fiber's molecular structure when subjected to force. On the other hand, the short -CH2-CH2- alkyl chain in 3,4-dihydroxyphenylpropionic acid can drive the cross-linked viscose fibers to recover through internal rotational restoring force after the external force is removed. On the other hand, 3,4-dihydroxyphenylpropionic acid can chemically cross-link with modified polyester fibers and viscose fibers to form a cross-linked network structure, effectively inhibiting fiber slippage, thereby enhancing the wrinkle-free properties of the polyester-viscose fibers in various aspects, and without producing harmful byproducts such as formaldehyde.

[0032] 2. The polyester fiber in the wrinkle-free and skin-friendly polyester-viscose fabric of the present application has been hydrophilically modified. On the one hand, it can form chemical cross-links with 3,4-dihydroxyphenylpropionic acid to increase the wrinkle-free property of the polyester-viscose fabric; on the other hand, after the hydrophilic modification, the hygroscopicity of the polyester fiber is increased. At the same time, the blending of polyester fibers with special cross-sections and viscose fibers can facilitate water evaporation and increase the moisture-wicking property of the fabric, thereby increasing the comfort and skin-friendliness of the polyester-viscose fabric. DETAILED DESCRIPTION

[0033] Preparation example of modified polyester fiber

[0034] Preparation Example 1: A modified polyester fiber was prepared according to the following method:

[0035] 1 kg of triangular cross-section polyester fiber was immersed in 2 kg of 2% by mass acetic acid aqueous solution for swelling treatment, and the fiber was taken out after soaking for 30 minutes.

[0036] 0.2 kg of maleic acid and 0.003 kg of azobisisobutyronitrile were added to 2 kg of deionized water and stirred to obtain a grafting solution. Under nitrogen atmosphere, the swollen polyester fiber was immersed in the grafting solution, the solution temperature was adjusted to 35°C, and the mixture was stirred for 2 hours, then washed with deionized water and dried to obtain the modified polyester fiber.

[0037] The specification of the triangular cross-section polyester fiber is FDY 150D / 36F.

[0038] Preparation Example 2: A modified polyester fiber was prepared according to the following method:

[0039] 1 kg of triangular cross-section polyester fiber was immersed in 1.5 kg of 2% by mass acetic acid aqueous solution for swelling treatment, and the fiber was taken out after soaking for 30 minutes.

[0040] 0.15 kg of maleic acid and 0.002 kg of azobisisobutyronitrile were added to 2 kg of deionized water and stirred to obtain a grafting solution. Under nitrogen atmosphere, the swollen polyester fiber was immersed in the grafting solution, the solution temperature was adjusted to 35°C, and the mixture was stirred for 2 hours, then washed with deionized water and dried to obtain the modified polyester fiber.

[0041] Preparation Example 3: A modified polyester fiber was prepared according to the following method:

[0042] 1 kg of triangular cross-section polyester fiber was immersed in 2 kg of 2% by mass acetic acid aqueous solution for swelling treatment, and the fiber was taken out after soaking for 30 minutes.

[0043] 0.25 kg of maleic acid and 0.004 kg of azobisisobutyronitrile were added to 2 kg of deionized water and stirred to obtain a grafting solution. Under nitrogen atmosphere, the swollen polyester fiber was immersed in the grafting solution, the solution temperature was adjusted to 35°C, and the solution was stirred for 2 hours, then washed with deionized water and dried to obtain the modified polyester fiber.

[0044] Preparation Example 4, a modified polyester fiber, is different from Preparation Example 1 only in that the amount of maleic acid added is 0.1 kg.

[0045] Preparation Example 5, a modified polyester fiber, is different from Preparation Example 1 only in that the polyester fiber with a triangular cross-section is not subjected to swelling treatment.

[0046] Preparation Example 6, a modified polyester fiber, is different from Preparation Example 1 only in that an equal amount of polyester fibers with circular cross-sections are used to replace the polyester fibers with triangular cross-sections.

[0047] Example

[0048] Example 1, a non-ironing skin-friendly polyester-viscose fabric, the preparation method is as follows:

[0049] 6.5 kg of the modified polyester fiber prepared in Preparation Example 1 and 3.5 kg of viscose fiber were blended to prepare a polyester-viscose fabric.

[0050] Add 0.8 kg of 3,4-dihydroxyphenylpropionic acid and 0.008 kg of azobisisobutyronitrile to 100 kg of deionized water and stir until evenly mixed to obtain a finishing agent aqueous solution. Immerse the resulting polyester-viscose fabric in the finishing agent aqueous solution at a temperature of 40 degrees Celsius for 70 minutes.

[0051] The impregnated polyester-viscose fabric is dried at 75° C. for 20 minutes, and then the dried fabric is baked at 120° C. for 4 minutes to obtain a wrinkle-free, skin-friendly polyester-viscose fabric.

[0052] Example 2, a wrinkle-free skin-friendly polyester-viscose fabric, the preparation method is as follows:

[0053] 6.7 kg of the modified polyester fiber prepared in Preparation Example 2 and 3.3 kg of viscose fiber were blended to prepare a polyester-viscose fabric.

[0054] Add 1 kg of 3,4-dihydroxyphenylpropionic acid and 0.01 kg of azobisisobutyronitrile to 150 kg of deionized water and stir until evenly mixed to obtain a finishing agent aqueous solution. Immerse the resulting polyester-viscose fabric in the finishing agent aqueous solution at a temperature of 40 degrees Celsius for 70 minutes.

[0055] The impregnated polyester-viscose fabric is dried at 75°C for 20 minutes, and then the dried fabric is baked at 120°C for 4 minutes to obtain a wrinkle-free and skin-friendly polyester-viscose fabric.

[0056] Example 3, a wrinkle-free skin-friendly polyester-viscose fabric, the preparation method is as follows:

[0057] 6.3 kg of the modified polyester fiber prepared in Preparation Example 3 and 3.7 kg of viscose fiber were blended to prepare a polyester-viscose fabric.

[0058] Add 0.6 kg of 3,4-dihydroxyphenylpropionic acid and 0.006 kg of azobisisobutyronitrile to 100 kg of deionized water and stir until evenly mixed to obtain a finishing agent aqueous solution. Immerse the resulting polyester-viscose fabric in the finishing agent aqueous solution at a temperature of 40 degrees Celsius for 70 minutes.

[0059] The impregnated polyester-viscose fabric is dried at 75° C. for 20 minutes, and then the dried fabric is baked at 120° C. for 4 minutes to obtain a wrinkle-free, skin-friendly polyester-viscose fabric.

[0060] Example 4, a wrinkle-free, skin-friendly polyester-viscose fabric, differs from Example 1 only in that the added amount of 3,4-dihydroxyphenylpropionic acid is 0.4 kg.

[0061] Example 5, a wrinkle-free, skin-friendly polyester-viscose fabric, differs from Example 1 only in that the modified polyester fiber prepared in Preparation Example 1 is replaced by an equal amount of the modified polyester fiber prepared in Preparation Example 4.

[0062] Example 6, a wrinkle-free, skin-friendly polyester-viscose fabric, differs from Example 1 only in that the modified polyester fiber prepared in Preparation Example 1 is replaced by an equal amount of the modified polyester fiber prepared in Preparation Example 5.

[0063] Example 7, a wrinkle-free, skin-friendly polyester-viscose fabric, differs from Example 1 only in that the modified polyester fiber prepared in Preparation Example 1 is replaced by an equal amount of the modified polyester fiber prepared in Preparation Example 6.

[0064] Comparative Example

[0065] Comparative Example 1 is a wrinkle-free, skin-friendly polyester-viscose fabric. The only difference from Example 1 is that the modified polyester fiber prepared in Preparation Example 1 is replaced by an equal amount of triangular cross-section polyester fiber (specification: FDY 150D / 36F) that has not undergone modified grafting treatment.

[0066] Comparative Example 2, a wrinkle-free, skin-friendly polyester-viscose fabric, differs from Example 1 only in that the polyester-viscose fabric is not finished with 3,4-dihydroxyphenylpropionic acid, that is, the polyester-viscose fabric is blended with 6.5 kg of the modified polyester fiber prepared in Preparation Example 1 and 3.5 kg of viscose fiber.

[0067] Performance testing

[0068] 1. Easy-to-iron performance test: The polyester-viscose fabrics prepared in Examples 1-7 and Comparative Examples 1-2 were tested for easy-to-iron performance according to GB / T 18863-2002, "Easy-to-iron Textiles." The smoothness after washing and drying was tested according to GB / T 13769-2009, "Textiles - Test Method for Smoothness of Fabric Appearance After Washing." Washing and drying were performed according to GB / T 8629-2017, "Textile Testing - Household Washing and Drying Procedure." The easy-to-iron performance of the fabrics was compared by evaluating their smoothness after five washes and drying cycles.

[0069] 2. Skin affinity test:

[0070] (1) The moisture permeability of the polyester-viscose fabrics prepared in Examples 1 to 7 and Comparative Examples 1 to 2 was tested in accordance with GB / T 12704.2-2009 "Test method for moisture permeability of textile fabrics - Part 2: Evaporation method". The moisture permeability of the fabric was expressed by calculating the water vapor mass passing vertically through the sample per unit area within a specified time.

[0071] (2) The air permeability of the polyester-viscose fabrics prepared in Examples 1 to 7 and Comparative Examples 1 to 2 was tested according to GB / T 5453-1997 “Determination of Air Permeability of Textile Fabrics”. The air permeability of the fabric was expressed by measuring the air flow rate vertically passing through a given area of ​​the fabric within a certain period of time and calculating the air permeability.

[0072] Characterize the skin-friendliness of fabrics based on moisture permeability and air permeability.

[0073] The experimental results are shown in Table 1:

[0074] Table 1 Results of the non-ironing and skin-friendly test

[0075]

[0076]

[0077] According to Table 1, in combination with Example 1 and Comparative Example 1, it can be seen that the smoothness of the appearance of Comparative Example 1 is reduced, and the moisture permeability and air permeability of the fabric are significantly reduced, indicating that the non-ironing property of Comparative Example 1 is reduced compared to Example 1, and the skin-friendliness of the fabric is significantly reduced. This may be because the polyester fiber in Comparative Example 1 has not been hydrophilically modified. On the one hand, the surface of the unmodified polyester fiber has no hydrophilic groups, resulting in poor hygroscopicity and poor air permeability. Sweat cannot be absorbed and evaporated by the fabric in a timely manner, and the skin-friendliness is reduced. On the other hand, the polyester fiber has not been hydrophilically modified, and there are no active groups on the surface that can cross-link with 3,4-dihydroxyphenylpropionic acid. The fiber structure of the polyester-viscose fabric lacks the retardation effect of cross-linking. Under the action of external force, the possibility of slippage increases, and the non-ironing property of the fabric is reduced.

[0078] Combining Example 1 and Comparative Example 2, it can be seen that the smoothness of the appearance of Comparative Example 2 is significantly reduced, and the moisture permeability and air permeability of the fabric are also reduced. This indicates that the non-ironing properties of Comparative Example 2 are significantly reduced compared to Example 1, and the skin-friendliness is reduced. This may be because the polyester-viscose fabric in Comparative Example 2 has not been finished with a 3,4-dihydroxyphenylpropionic acid finishing agent. Without the penetrating finishing of 3,4-dihydroxyphenylpropionic acid, on the one hand, the rigid structure of the benzene ring is lacking, and a cross-linked network structure cannot be formed between the fiber molecules of the polyester-viscose fabric. When the polyester-viscose fabric is subjected to external force, the fiber molecules are easily displaced and difficult to recover after the external force is removed, significantly reducing the non-ironing properties of the polyester-viscose fabric. On the other hand, the lack of support from the short alkyl chains reduces the elasticity of the fabric, and the skin-friendliness of the fabric is also reduced.

[0079] Combining Examples 1, 2, and 3, it can be seen that the smoothness, moisture permeability, and air permeability of Examples 2 and 3 do not change significantly compared to Example 1, indicating that the wrinkle-free properties and skin-friendliness of Examples 2 and 3 are similar to those of Example 1. This may be because the raw material ratios in Examples 2 and 3 are varied within the required range, indicating that varying the raw material mass ratio within the required range has no significant effect on the wrinkle-free properties and skin-friendliness of the fabric.

[0080] Comparing Examples 1 and 4, it can be seen that Example 4 exhibits a slight decrease in appearance smoothness, as well as a slight decrease in the moisture and air permeability of the fabric. This indicates that Example 4 exhibits slightly lower iron-free properties and skin-friendliness compared to Example 1. This may be due to the reduced amount of 3,4-dihydroxyphenylpropionic acid added during the finishing process of Example 4, which reduces the crosslinking between the fiber molecules of the polyester-viscose fabric and decreases the concentration of benzene rings in the fabric. This results in a lack of a crosslinked network and the blocking effect of the benzene rings, increasing the likelihood of slippage when subjected to external forces, leading to a decrease in iron-free properties.

[0081] Combining Examples 1, 5, and 6, it can be seen that the smoothness of the appearance of Examples 5 and 6 does not change significantly compared to Example 1, while the moisture permeability and air permeability of the fabrics decrease. This indicates that the wrinkle-free properties of Examples 5 and 6 are similar to those of Example 1, while the skin-friendliness of Examples 5 and 6 decreases compared to Example 1. This may be because, in Example 5, the amount of dicarboxylic acid vinyl compound added to the polyester fiber during the modification and grafting process is reduced, resulting in a decrease in the amount of grafted monomers; and in Example 6, the polyester fiber is not subjected to a swelling treatment before modification and grafting, and the gaps between the molecular structures of the polyester fiber are not increased due to the swelling effect. Both of these factors result in a decrease in the grafting rate of the polyester fiber after modification and grafting, and a decrease in the number of hydrophilic groups grafted onto the polyester fiber surface, thereby reducing the hygroscopicity of the polyester-viscose fabric and the skin-friendliness of the fabric.

[0082] Combining Examples 1 and 7, it can be seen that the smoothness of Example 7 is not significantly different from that of Example 1, while the moisture permeability and air permeability of the fabric have decreased. This indicates that the wrinkle-free properties of Example 7 are similar to those of Example 1, but the skin-friendliness of Example 7 has decreased compared to Example 1. This may be because Example 7 uses polyester fibers with circular cross-sections. Compared to polyester fibers with irregular cross-sections, polyester fibers with circular cross-sections cannot form gaps that facilitate water evaporation when blended with viscose fibers. The elastic modulus of the polyester fibers also decreases, resulting in reduced skin-friendliness of the fabric.

[0083] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make non-creative modifications to the present embodiment as needed, but as long as they are within the scope of the claims of the present application, they are protected by the patent law.

Claims

1. A non-ironing skin-friendly polyester-viscose fabric, which is obtained by blending polyester fiber and viscose fiber and finishing it, characterized in that: The wrinkle-free and skin-friendly polyester-viscose fabric is grafted with 3,4-dihydroxyphenylpropionic acid through an esterification reaction during the finishing process; The polyester fiber is a polyester fiber with a special cross-section, and the mass ratio of the polyester fiber to the viscose fiber is (63-76):(33-37); the polyester fiber is a modified polyester fiber grafted with a dicarboxy vinyl compound; the dicarboxy vinyl compound includes one or more of maleic acid, fumaric acid, glutaric acid, and hexadienedioic acid; the raw materials of the modified polyester fiber include polyester fiber, dicarboxy vinyl compound, and initiator in a mass ratio of 100:(15-25):(0.2-0.5); The modified grafting steps of the modified polyester fiber are as follows: immersing the polyester fiber in a swelling agent for swelling treatment; adding an initiator and a dicarboxyl vinyl compound to deionized water and stirring and mixing to obtain a grafting solution; under the protection of an inert gas atmosphere, immersing the swollen polyester fiber in the grafting solution, adjusting the solution temperature to 30-40° C., stirring and reacting for 2-3 hours, and then washing with water to obtain the modified polyester fiber; During the finishing process, the mass ratio of polyester-viscose fabric, 3,4-dihydroxyphenylpropionic acid and esterification reaction catalyst is 100: (6-10): (0.04-0.12), and the esterification reaction catalyst includes one or more of thionyl chloride, p-toluenesulfonic acid, sodium acetate and potassium hydrogen sulfate.

2. The method for preparing a non-ironing skin-friendly polyester-viscose fabric according to claim 1, characterized in that: The steps include: Finishing and modification: the polyester fiber is modified and blended with the viscose fiber to obtain a polyester-viscose fabric, and the polyester-viscose fabric is impregnated and finished, and an esterification reaction is performed to obtain an impregnated polyester-viscose fabric; Heat setting: Dry the impregnated polyester-viscose fabric at 70-80°C for 15-20 minutes; bake the dried fabric at 115-125°C for 3-5 minutes to obtain the non-ironing skin-friendly polyester-viscose fabric.