Electrochromic device with multiple electrochromic layers

By using multiple cross-linked electrochromic layers and adjusting the film thickness in electrochromic devices, combined with cross-linking agents and optical modeling technology, the problems of limited color selection pools and intermediate colors in the existing technology are solved, and rich colors are achieved. Wheel and multi-color capabilities simplify device design.

CN116472490BActive Publication Date: 2024-10-11AMBILIGHT INC
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
CN202180076944.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2020-11-16
Filing Date
2021-07-15
Publication Date
2024-10-11
Estimated Expiration
2041-07-15

AI Technical Summary

Technical Problem

Existing electrochromic devices have a limited color selection pool for full-color display and information expression, and are susceptible to undesirable intermediate colors and phase separation when color mixing is performed by physically mixing electrochromic polymers, resulting in complex device structure design and Material selection dilemma.

Method used

Using multiple cross-linked electrochromic layers, by adjusting the film thickness and material selection of each electrochromic layer, full-color coloring and multi-color capabilities are achieved, and cross-linking agents and optical modeling technology are used to optimize the electrochromic layer. Solvent resistance and optical properties, reducing intermediate colors.

Benefits of technology

A rich color wheel and multi-color capabilities are achieved, intermediate colors are reduced, the performance and manufacturing flexibility of electrochromic devices are improved, and the device structure design is simplified.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116472490B_ABST
    Figure CN116472490B_ABST
Patent Text Reader

Abstract

An electrochromic device has multiple electrochromic layers stacked in sequence, wherein the lower electrochromic layers are crosslinked. The crosslinked electrochromic layers are solution processable without compromising their optical and electrochromic properties. The disclosed electrochromic device can produce a full color palette with minimized intermediate colors and demonstrates multicolor capabilities. Multilayer electrochromic polymer patterns with surface texture information are fabricated. Methods for controlling electrochromism or multicolor electrochromism are discussed.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to electrochromic devices having multiple electrochromic layers, devices incorporating electrochromic devices, and methods of controlling the electrochromic or multi-color electrochromicity of electrochromic devices. Background Art

[0002] Expanding the color selection pool of electrochromic devices (ECDs) is crucial for their widespread application in full-color display and information expression. The full-color palette of electrochromic polymers (ECPs) can be achieved by adjusting the molecular structure by chemical synthesis or mixing various ECPs with primary colors based on subtractive color methods. However, due to high synthesis requirements and the complex relationship between polymer structure and color, the synthesis method of changing the main chain or side chain is complicated and time-consuming. Color mixing by physically mixing various ECPs with primary colors is affected by undesirable intermediate colors and phase separation. In addition, conventional multicolor electrochromic devices usually require complex device structure design or difficult EC material selection. Therefore, it is highly desirable to develop an ECD that can not only produce a full-color palette, but also produce multicolor capabilities in an easy and flexible form. Summary of the invention

[0003] An electrochromic device is described herein, comprising: a first transparent electrode; a plurality of electrochromic layers sequentially stacked on the first transparent electrode, wherein an upper electrochromic layer is disposed on a lower electrochromic layer; an ion storage layer disposed on the electrochromic layer; and a second transparent electrode disposed on the ion storage layer. The lower electrochromic layer comprises a cross-linked electrochromic layer that exhibits solvent resistance to a solvent used in the upper electrochromic layer.

[0004] In some embodiments, an uppermost one of the electrochromic layers is cross-linked.

[0005] Crosslinking of the electrochromic layer occurs with or without a crosslinking agent.

[0006] The film thickness of each electrochromic layer is adjusted to achieve different colors.

[0007] Different electrochromic layers with different electrochromic materials are selected to achieve different colors.

[0008] In some embodiments, the disclosed electrochromic devices include a layer having a cyan electrochromic polymer, a layer having a magenta electrochromic polymer, and a layer having a yellow electrochromic polymer.

[0009] In some embodiments, the disclosed electrochromic device presents a black color with minimized intermediate colors. The black electrochromic device includes a layer of a cyan electrochromic polymer as a bottom layer, a layer of a magenta electrochromic polymer as a top layer, and a layer of a yellow electrochromic polymer inserted between the bottom layer and the top layer. The film thickness ratio of the three color layers from bottom to top is 25:8:10.

[0010] The present invention also relates to an electronic device incorporating the disclosed electrochromic device.

[0011] In some embodiments, an electronic device includes a multi-layer electrochromic polymer pattern having surface texture information.

[0012] In another aspect, a method for controlling electrochromism or multi-color electrochromism of an electrochromic device having multiple electrochromic layers is provided. The method includes adjusting the electrochromic material and thickness of each electrochromic layer. BRIEF DESCRIPTION OF THE DRAWINGS

[0013] Certain features of various embodiments of the present technology are set forth in detail in the appended claims. A better understanding of the features and advantages of the present technology will be obtained by reference to the following detailed description and the following drawings, which set forth illustrative embodiments and in which the principles of the invention are utilized. For the purpose of illustrating the invention, the accompanying drawings show aspects of one or more embodiments of the invention. It should be understood, however, that the invention is not limited to the precise arrangements and instrumentalities shown in the drawings.

[0014] Figure 1 is a simplified structure of an electrochromic (EC) layer disclosed herein having multiple EC layers according to an example embodiment.

[0015] Figure 2 is a scanning electron micrograph of an example dual-layer ECD disclosed herein, according to an example embodiment.

[0016] Figure 3 is a graph illustrating the insoluble fraction (%) of ECP-Magenta (ECP-M) cross-linked with the cross-linker bis(fluorophenyl azide) (bisFA) at different cross-linker weight percentages according to various embodiments.

[0017] Figure 4 is a graph illustrating the insoluble fraction (%) of ECP-M cross-linked with the cross-linking agent bisFA after different cross-linking times according to various embodiments.

[0018] Figure 5 are Fourier transform infrared (FTIR) spectra of the ECP-M layer before and after cross-linking at a wavelength of 2050-2250 nm.

[0019] Figure 6(A) to Figure 6(B) are the absorption spectra of cross-linked ECP-yellow (ECP-Y) ( FIG. 6(A) ) and ECP-cyan (ECP-C) ( FIG. 6(B) ) before and after chloroform washing.

[0020] Figure 7(A) to Figure 7(D) The optical and electrochemical properties of example ECP-M layers with and without optimized crosslinking are shown. Figure 7(A) shows cyclic voltammetry (CV) data; Figure 7(B) shows the absorption spectrum in the colored state; Figure 7(C) shows the full wavelength transmission spectrum in the colored and faded states; Figure 7(D) is a graph illustrating the switching kinetics.

[0021] Figure 8(A) to Figure 8(C) The optical and electrochemical properties of example ECP-C layers with and without optimized crosslinking are shown. Figure 8(A) is CV data; Figure 8(B) shows full wavelength transmission spectra in the tinted and faded states; Figure 8(C) is a graph illustrating the switching kinetics.

[0022] Figure 9(A) to Figure 9(C) The optical and electrochemical performance of example ECP-Y layers with and without optimized crosslinking are shown. Figure 9(A) shows CV data; Figure 9(B) shows full wavelength transmission spectra in the tinted and faded states; Figure 9(C) is a graph illustrating the switching kinetics.

[0023] Fig.10 A workflow scheme for optical modeling of a multi-layer ECP stack according to an example embodiment is illustrated.

[0024] Figure 11(A) to Figure 11(C) 11(A) , ECP-M ( FIG. 11(B) ), and ECP-Y ( FIG. 11(C) ) according to various embodiments are graphs illustrating the correlation between the thickness and the concentration.

[0025] Figure 12(A) to Figure 12(C) Contains experimental and modeled spectra of bilayer ECP stacks with various polymer thicknesses according to various embodiments. Figure 12(A) is for a 190nm ECP-M layer stacked with a 210nm ECP-C layer; Figure 12(B) is for a 210nm ECP-C layer stacked with a 160nm ECP-Y layer; Figure 12(C) is for a 190nm ECP-M layer stacked with a 160nm ECP-Y layer.

[0026] Figure 13(A) to Figure 13(C)Contains transmission spectra of experimentally reconstructed bilayer ECP stacks according to various embodiments. Figure 13 (A) is for a 190nm ECP-M layer superimposed on a 210nm ECP-C layer; Figure 13 (B) is for a 210nm ECP-C layer superimposed on a 160nm ECP-Y layer; Figure 13 (C) is for a 190nm ECP-M layer superimposed on a 160nm ECP-Y layer.

[0027] Figure 14(A) to Figure 14(I) are images of example double-layer ECP stack films with different colors according to various embodiments. Figure 14(A) is an image of a lower cross-linked layer prepared from 18 mg / ml ECP-C and a top layer prepared from 30 mg / ml ECP-Y; Figure 14(B) is an image of a lower cross-linked layer prepared from 36 mg / ml ECP-C and a top layer prepared from 30 mg / ml ECP-Y; Figure 14(C) is an image of a lower cross-linked layer prepared from 72 mg / ml ECP-C and a top layer prepared from 30 mg / ml ECP-Y; Figure 14(D) is an image of a lower cross-linked layer prepared from 50 mg / ml ECP-C and a top layer prepared from 30 mg / ml ECP-M; Figure 14(E) is an image of a lower cross-linked layer prepared from 50 mg / ml ECP-C and a top layer prepared from 10 mg / ml ECP-M; Figure 14(F) is an image of a lower cross-linked layer prepared from 50 mg / ml ECP-C and a top layer prepared from 5 mg / ml Figure 14(G) is an image of a lower cross-linked layer prepared by 10 mg / ml ECP-Y and a top layer prepared by 40 mg / ml ECP-M; Figure 14(H) is an image of a lower cross-linked layer prepared by 20 mg / ml ECP-Y and a top layer prepared by 40 mg / ml ECP-M; Figure 14(I) is an image of a lower cross-linked layer prepared by 30 mg / ml ECP-Y and a top layer prepared by 10 mg / ml ECP-M.

[0028] Figure 15(A) to Figure 15(B) Cyclic voltammetry data according to various embodiments are illustrated. FIG. 15(A) is for ECPs mixing, and FIG. 15(B) is for ECPs stacking.

[0029] Figure 16(A) to Figure 16(B) Transmittance evolution data monitored at 490 nm and 600 nm as a function of applied voltage according to various embodiments are illustrated. FIG. 16(A) is for ECPs mixing, and FIG. 16(B) is for ECPs stacking.

[0030] Figure 17(A) to Figure 17(B)17(A) illustrates the transmission spectrum; FIG. 17(B) illustrates the dual potential step timing absorption data. The inset in FIG. 17(B) is an image of an example three-layer ECP stack film according to an example embodiment, which shows a black color with minimal intermediate colors in the tinted and faded states.

[0031] Figure 18(A) to Figure 18(B) 18(A) is an image of an example multilayer electrochromic pattern with a layered texture; FIG18(B) is a 2D height map image measured by an optical profilometer, as shown in the dashed box portion in FIG18(A); FIG18(C) is a profile showing height variation extracted along the dashed line shown in FIG18(B).

[0032] Figure 19(A) to Figure 19(B) 19(A) is at -0.2V; FIG. 19(B) is at 0.7V; and FIG. 19(C) is at 1.2V.

[0033] Figure 20(A) to Figure 20(B) are images of two example bilayer ECP stack films. FIG20(A) is for an example film having a crosslinked ECP-Y layer beneath a top ECP-M layer. FIG20(B) is for an example film having a crosslinked ECP-C layer beneath a top ECP-M layer.

[0034] Fig.21 Shows Figure 20(A) to Figure 20(B) UV-Vis spectra of two example bilayer ECP film stacks are shown.

[0035] Figure 22(A) to Figure 20(B) are images of two example bilayer ECP film stacks. FIG. 22(A) is for a thicker ECP-Y layer beneath a thinner top ECP-M layer; FIG. 22(B) is for a thinner ECP-Y layer beneath a thicker top ECP-M layer.

[0036] Fig.23 yes Figure 22(A) to Figure 20(B) UV-Vis spectra of two example bilayer ECP film stacks are shown. DETAILED DESCRIPTION

[0037] In the following description, certain specific details are set forth in order to provide a thorough understanding of various embodiments of the present invention. However, it will be appreciated by those skilled in the art that the present invention can be implemented without these details. Moreover, although various embodiments of the present invention are disclosed herein, many adaptations and modifications may be made within the scope of the present invention according to the common knowledge of those skilled in the art. These modifications include replacing any aspect of the present invention with known equivalents in order to achieve the same results in substantially the same manner.

[0038] Unless the context requires otherwise, in this specification and claims, the word "comprise" and variations thereof (e.g., "comprising" and "containing") are to be interpreted in an open, inclusive sense, i.e., "including, but not limited to." Recitation of numerical ranges throughout the specification is intended to serve as a shorthand notation for individually referring to each individual value falling within the range, including the values ​​defining the range, and each individual value is incorporated into the specification as if it were individually recited herein. In addition, the singular forms "a," "an," and "the" include plural references unless the context clearly dictates otherwise.

[0039] References in this specification to "one embodiment" or "an embodiment" mean that a particular feature, structure, or characteristic described in conjunction with the embodiment is included in at least one embodiment of the present invention. Thus, the phrases "in one embodiment" or "in an embodiment" appearing in various places in this specification do not necessarily all refer to the same embodiment, but may refer to the same embodiment in some cases. Furthermore, the particular features, structures, or characteristics may be combined in any suitable manner in one or more embodiments.

[0040] In this specification, three specific electrochromic polymers are used for the purpose of illustration. It should be understood that the present invention is not limited to these examples. ECP-magenta (ECP-M) is a magenta ECP having the chemical formula 1 listed below. ECP-yellow (ECP-Y) is a yellow ECP having the chemical formula 2 listed below. ECP-cyan (ECP-C) is a cyan ECP having the chemical formula 3 listed below.

[0041]

[0042] This specification discloses an example electrochromic device including a plurality of electrochromic (EC) layers stacked in sequence, wherein an upper electrochromic layer is disposed on top of a lower electrochromic layer, and the lower electrochromic layer is cross-linked and exhibits solvent resistance to solvents used, for example, in the upper electrochromic layer or other layers generally adjacent to the cross-linked electrochromic layer.

[0043] The cross-linked electrochromic layer can resist the solvent used in the layer immediately above or immediately below the cross-linked electrochromic layer, which layer can be another electrochromic layer or other layers. The solvent resistance of the resulting cross-linked ECPs can avoid the dissolution problem faced by the lower polymer layer during the coating process of the upper polymer, so that multiple electrochromic layers can be arranged in the solution. The disclosed stacking process is compatible with various printing methods and makes the manufacture of multilayer structures feasible. In addition, the cross-linked ECPs do not sacrifice their optical and electrochemical properties, thereby allowing the disclosed ECDs to achieve good performance as expected. The ECD disclosed herein can generate secondary or more complex colors, which not only enrich the color wheel but also allow multicolor capabilities to be achieved. In addition, the ECD disclosed herein can efficiently minimize intermediate colors, which are usually difficult to avoid when using polymer mixing technology.

[0044] Figure 1 An example layer stacking scheme of the present invention is shown in . The ECD disclosed herein has n electrochromic (EC) layers (1st-nth EC layers). The nth layer is the top layer, and the other layers are lower EC layers. Each EC layer can be directly arranged on a previously cross-linked EC layer. All lower EC layers are cross-linked, while the nth layer can be cross-linked or uncross-linked. The solvent-resistant electrochromic layer makes the stacking of EC layers feasible. Figure 2 Shown is a microscopic image of an example double-layer ECP thin film stack on a substrate, which is formed by successfully disposing one EC layer (eg, ECP-layer 2) on top of another cross-linked EC layer (eg, ECP-layer 1).

[0045] Cross-linking of the cross-linked EC layer can occur with or without a cross-linking agent. The type of cross-linking and the choice of cross-linking agent depend on the chemical composition and chemical structure of the EC material from that particular layer. In some embodiments, the EC layer is cross-linked without a cross-linking agent. For example, the EC material, polysilsesquioxane containing triarylamine, can be self-cross-linked by forming a silsesquioxane cage at 180° C. in an argon atmosphere for 1 hour during thin film processing. In some embodiments, the EC layer is cross-linked with a cross-linking agent. For example, ECP-fuchsin can be cross-linked using the cross-linking agent bis(fluorophenyl azide) (bisFA). The cross-linking agent is mixed with the ECP-fuchsin / chloroform solution at a ratio of 5 wt % (cross-linking agent: ECP-fuchsin) and treated with ultraviolet (UV) light for 5 minutes after the thin film process. The selected cross-linking can improve the resistance of the particular electrochromic layer to solvents used for subsequent thin film processing without significantly affecting the electrochromic and electrochemical properties of the cross-linked electrochromic layer for its designed application.

[0046] Cross-linking condition optimization and impact assessment

[0047] The cross-linking efficiency can affect the degree of solvent resistance of the EC layer. When a certain cross-linking agent is selected, the parameters that affect the degree of cross-linking include the cross-linking agent concentration and the cross-linking time. In order to explore the optimal cross-linking conditions, the insoluble fraction is quantified to monitor the cross-linking efficiency. The insoluble fraction is determined by the maximum absorbance in the visible light range before and after solvent washing of a specific EC layer and is quantified using Equation 1.

[0048]

[0049] To demonstrate how to study photo-crosslinking conditions, ECP-M was used as an example ECP for the EC layer to be crosslinked, and BisFA was used as an example crosslinker. Chloroform was used to test solvent resistance before and after crosslinking, which is a common polymer processing solvent. UV light treatment after the film process was used for crosslinking. BisFA was mixed with an ECP-M / chloroform solution with 0wt% to 9wt% crosslinker (crosslinker: ECP-M). The spin-cast film from the blend was exposed to UV light for a time range of 0-10min in a nitrogen atmosphere to complete the crosslinking. The crosslinked film was then immersed in chloroform for 5 minutes and then further washed with chloroform.

[0050] Both cross-linking agent concentration and cross-linking time were studied. Figure 3 As shown, the insoluble fraction (%) of different crosslinker weight percentages is compared. When the crosslinker weight percentage is less than 5%, the EC layer has a low insoluble fraction (<20%), and when the crosslinker weight percentage is equal to or higher than 5%, the insoluble fraction reaches a plateau of at least 85%. This indicates that for this system, the optimal crosslinker weight percentage is 5wt%. Figure 4 The insoluble fraction (%) for different UV treatment times is shown in . After 4 minutes of UV treatment, the insoluble fraction reached a stable level of at least 85%. In order to avoid significant polymer conformational changes caused by prolonged UV treatment, an optimal cross-linking time of 5 minutes was selected.

[0051] The successful cross-linking of the ECP-M layer was further confirmed by comparing the FTIR spectra before and after cross-linking under the optimized conditions and with an exemplary cross-linker bisFA (5 wt% cross-linker, UV treatment for 5 min). Figure 5 As shown, the loss of N3 (NN stretch) indicates successful cross-linking within the ECP-M layer.

[0052] The same optimal cross-linking conditions can be applied to prepare other cross-linked electrochromic materials, for example, ECP-C as shown in Figure 6(A) and ECP-Y as shown in Figure 6(B). After cross-linking with 5wt% bisFA and UV treatment for 5 minutes, both ECP-C and ECP-Y obtained more than 98% insoluble fraction.

[0053] Crosslinking has little effect on the electrochromic and optical properties of the crosslinked electrochromic layer. Figure 7(A) to Figure 7(D) As shown in Figure 2, compared with pure ECP-M, cross-linked ECP-M exhibited almost the same CV, absorbance in the colored state, full wavelength transmittance in the colored and faded states, and optical contrast (the difference in transmittance of ECP at 550nm between the colored and faded states), while maintaining similar switching kinetics. Figure 8(A) to Figure 8(C) and Figure 9(A) to Figure 9(C) As shown, the other two primary color ECPs (ECP-C and ECP-Y) also showed the same insignificant cross-linking effect.

[0054] Optical prediction

[0055] The insignificant effect of cross-linking on the electrochromic and optical properties of the cross-linked EC layers allows modeling and prediction of the spectral properties and coloration of individual EC layers. Thus, the optical properties of stacked EC layers are predictable, providing guidance for possible ECD design and fabrication. Fig.10 The workflow for optical modeling of the disclosed electrochromic device is shown in . A multilayer geometry with a high aspect ratio is constructed to simulate a multilayer stacked ECP film. Depolarized electromagnetic waves with a wavelength of 400 to 800 nm in 10 nm steps are applied vertically from top to bottom to the geometry. The intrinsic values ​​of each polymer - refractive index, extinction coefficient and thickness - are applied to each layer of the model to study the interaction between the electromagnetic wave and the polymer stacking system. The transmission or reflection spectrum can be derived from the study results, from which the chromaticity value is extracted to predict the color rendering of the system.

[0056] To confirm that the predicted results match well with the experimental results, optical modeling of a double stack of ECP films in the colored state was performed. Since the concentration is controllable during the coating process, the relationship between thickness and concentration (e.g. Figure 11(A) to Figure 11(C) ) to generate the required thickness for modeling. Here, ECP-C, ECP-M, and ECP-Y are used as example ECPs for modeling. Note that the concentration-thickness relationship varies even for ECPs with the same chemical formula but different molecular weights. The three ECPs are combined in pairs to generate three bilayer stacking scenarios in the simulation, as shown in Figure 12(A) to Figure 12(C) The thicknesses of ECP-C, ECP-M and ECP-Y were 210nm, 190nm and 160nm respectively. Based on the calculation results, the transmittance of three double-layer ECP stacked films was derived and Figure 12(A) to Figure 12(C) Based on the experimental results, the transmission spectrum of the double-layer ECP stack film is observed to be Figure 12(A) to Figure 12(C) Obviously, they are in good agreement with the modeled values ​​(dashed curve), indicating the validity of the modeling. Figure 12(A) to Figure 12(C)It is also shown that the colors from the experimental and modeled spectra are very similar. Figure 13(A) to Figure 13(C) As shown, the reconstructed double-layer ECP stack film shows a change in transmittance between the reduced (colored) and oxidized (faded) states, which demonstrates that the double-layer ECP stack film exhibits good electrochromic performance. After several oxidation and reduction cycles, a break-in effect can be observed for the three reconstructed stacked electrochromic films. This break-in effect can be predicted using the optical property values ​​of the break-in films through optical modeling (data not shown).

[0057] Successful optical modeling can be used to guide the design of an ECD with a specific color table by changing input parameters, including parameters about the material (e.g., refractive index, extinction coefficient, etc.) and the film thickness of each layer. The structure of the electrochromic material determines the neutral color to be displayed. The thickness of each EC layer can control the color saturation of each layer. Therefore, by adjusting the electrochromic material and thickness of each layer, the ECD disclosed in this article with multiple EC layers can produce a variety of colors that are difficult to produce for an ECD with only a single EC layer. Figure 14(A) to Figure 14(I) As shown in the various double-layer ECP stack films in , each film is made by stacking a lower cross-linked EC layer and a top EC layer with different thicknesses controlled by different concentrations. By varying the different ECPs and the different thicknesses of the various layers, a variety of colors can be achieved even for a double-layer film system. The thickness is controlled by the concentration of the ECP solution. The higher the concentration, the greater the thickness produced. ECPs with the same chemical formula but different molecular weights may have different concentration-thickness relationships, so the concentration value in one specific embodiment may not be directly applicable to another embodiment. ECDs with more EC layers are expected to produce richer colors. For example, Figure 14(A) to Figure 14(C) The various bilayer ECP stack films shown have different thicknesses of the lower ECP-C layer and the top ECP-Y layer, and the resulting colors vary from seaweed green in FIG. 14(A) to forest green in FIG. 14(B) to lime green in FIG. 14(C). Figure 14(D) to Figure 14(F) The various bi-layer ECP stack films shown have different thicknesses of the lower ECP-C layer and the top ECP-M layer, thus showing different colors. Figure 14(G) to Figure 14(I) The various bi-layer ECP stack films shown have different thicknesses of the lower ECP-Y layer and the top ECP-M layer, thereby showing different colors.

[0058] Widely absorbed black is a color widely accepted in the industry for various applications. In some embodiments, black can be produced by three different EC layers, including an ECP-C layer, an ECP-Y layer, and an ECP-M layer, wherein at least two EC layers closer to the electrodes are cross-linked. Since the sum of these three colors (cyan, yellow, and magenta) covers the entire spectrum well, the overall color of the ECD appears black. Regardless of the relative position between the three layers, the ECD displays black with slight variations. At the same time, different degrees of black can be achieved by adjusting the applied voltage and thickness.

[0059] Conventional polymer blending methods cannot avoid intermediate colors during conversion due to the difference in electrochromic onset potentials of the constituent ECPs. However, the ECDs disclosed herein can minimize intermediate colors. As shown in Figure 15 (A), when two ECPs (ECP-orange and ECP-blue) are mixed together, ECP-blue has a lower electrochromic onset potential, so it is oxidized first. The asynchronous doping process causes the ECP-blue layer with a lower onset potential to fade before the ECP-orange layer with a higher onset potential, thereby producing intermediate colors. Therefore, the cyclic voltammetry of the film presents two separate electrochemical onset potentials at about 0V and 0.7V (Figure 15 (A)), indicating the presence of asynchronous electrochemical doping and intermediate colors. However, the disclosed ECD only shows a single electrochemical onset potential at about 0.58V, indicating synchronized electrochemical reactions and color changes, thus resulting in minimal intermediate colors, as shown in Figure 15 (B). When two ECPs are stacked with ECP-orange at the top, electrons will be injected from the ECP-blue / ITO electrode interface, while ions diffuse from the ECP-orange / electrolyte interface at a positive potential. Only when ECP-orange is doped will the diffusion of ions become unhindered and enter the ECP-blue to complete the doping of the stack. FIG16 shows the spectral electrochemical performance at wavelengths of 490nm and 600nm, which are the maximum absorption peaks of ECP-blue and ECP-orange, respectively, as a function of applied voltage. Unlike conventional polymer blends (as shown in FIG16(A)), for the disclosed ECD, the transmittance of the electrochromic stack at 0.6V at 600nm and 490nm increases almost simultaneously, indicating a uniform color change (as shown in FIG16(B)). Therefore, intermediate colors can be minimized.

[0060] Example 1: Three-layer ECP stack black film with minimized intermediate colors

[0061] Black electrochromic materials have attracted great interest due to their wide range of applications. Neutral gray is the purest black, which contains approximately equal amounts of spectral colors. According to the CMY color model, when ECP-C, ECP-M, and ECP-Y are mixed and have equal color contributions, their mixture will display neutral gray. However, since these three ECPs have different absorption coefficients, their thickness ratios must be carefully adjusted to obtain neutral gray, which usually requires dedicated experimental labor.

[0062] In some embodiments, neutral gray can be obtained by stacking ECP-C, ECP-M, ECP-Y at an appropriate thickness ratio. Optical modeling shows that when the film thickness of ECP-C, ECP-M, ECP-Y is 250, 80, and 100 nm, respectively, the maximum absorption intensity of the three ECPs is almost the same, indicating a neutral gray. The actual thickness may not be an exact number for each layer, but it is required that the three EC layers have the same thickness ratio of 25:8:10. By changing the actual thickness while maintaining the same ratio, a lighter or darker shade of neutral gray / black is produced.

[0063] According to the modeling and concentration-thickness relationship, the three polymers were arranged in chloroform solutions with concentrations of 26 mg / mL, 11 mg / mL and 12 mg / mL on ITO / glass in the order of ECP-C / ECP-Y / ECP-M from bottom to top to prepare a neutral gray three-layer ECP stacked film. Figures 17(A) and 17(B) show the results of the spectral electrochemical and double potential step chronoabsorption measurements of the stacked polymers. A successful and stable color change between neutral gray and transparent was demonstrated. The three-layer ECP stacked film showed an optical contrast of 38% between the colored and faded states at 555nm, with a switching time of 9s.

[0064] Example 2: ECD with multi-layer electrochromic pattern and layered texture

[0065] The present invention also relates to a device incorporating the disclosed electrochromic device. In addition to facilitating the construction of color palettes and controlling intermediate colors, the ECP stacking technique also opens up a way to develop ECP patterns with layered textures, thereby stimulating a variety of potential applications such as sophisticated optoelectronic displays and counterfeit labels.

[0066] In some embodiments, the device includes a multilayer electrochromic polymer pattern with surface texture information. The multilayer ECP pattern is constructed by combining ECP stacking technology with photolithography to generate surface texture information. As shown in Figure 18 (A), the multilayer ECP pattern has an ECP-M rectangle as the bottom layer, a vertical ECP-Y line in the middle, and a layer of horizontal ECP-Y lines at the top. Therefore, the intersection of two ECP-Y lines and the ECP-M rectangle is a three-layer ECP stack. Specifically, a magenta rectangular pattern is first printed, which is covered on a spin-coated ECP-M film with a photomask containing a corresponding shape, and then the film is exposed to UV light for 5min. The area not covered by the photomask is cross-linked, and chloroform is used to wash off the remaining uncross-linked films. Similarly, two more layers of ECP-Y are spin-coated on the top of the ECP-M pattern in sequence, and a cross-linked line pattern is generated. After obtaining the multilayer pattern, an optical profilometer is used to map out the periodic representative structure in the pattern (as shown in the dashed box portion in Figure 18 (A)), as shown in Figure 18 (B), where the color code indicates the height of the ECP surface. Obviously, four different heights are observed on the film surface: the blue background is the ITO substrate surface, the green rectangle on the top of the substrate is the 1st layer ECP-M, the orange line on the top of the rectangle is the 2nd and 3rd layers ECP-Y, and the small red rectangle is the intersection of the three layers. The height profile of the film cross-section along the dashed line (as shown in Figure 18 (B)) was further extracted and shown in Figure 18 (C). The dashed line does not cross the 3rd layer ECP-Y line, so the thickness of the three-layer ECP stack is not shown. As shown in Figure 18 (C), the thickness of the rectangular pattern is about 200nm, and the thickness of the line pattern is about 400nm after subtracting the substrate thickness. This rich texture surface makes it suitable for a variety of potential applications, such as counterfeit printing or color texture display. Further, as Figure 19(A) to Figure 19(C) As shown, the electrochromism of the multilayer pattern was monitored under an optical microscope. At -0.2V (Figure 19 (A)), both ECP-M and ECP-Y are in a colored state, so that both the cubes and the lines have vivid colors. At 0.7V (Figure 19 (B)), ECP-M is oxidized, leaving only the line pattern visible. At 1.2V (Figure 19 (C)), both the lines and the cubes are faded. These voltage-dependent ECP patterns enhance the ability to express information, allowing for more versatile and intelligent color displays of ECP.

[0067] In another aspect, the present invention also provides a method for controlling the color and multi-color capability of the disclosed ECDs having multiple EC layers. The method includes adjusting the parameters of each electrochromic layer, including the electrochromic material and thickness of each layer.

[0068] To demonstrate the ability to control the color and multicolor capabilities of the disclosed ECDs, different bilayer ECP stack films were used as examples. The lower EC layer, closer to the electrode, was cross-linked. To achieve this, the ECP solution that formed the lower EC layer also included 4 wt% bisFA as a cross-linking agent. The cross-linking process was performed by irradiating the film under UV light for 5 minutes in a N2-filled glove box before spin-coating the top EC layer on top of the lower EC layer. The top EC layer, further away from the electrode, was not cross-linked.

[0069] EC Materials

[0070] Different colors can be obtained by combining EC materials with different colors, such as Figure 20(A) to Figure 20(B) Two double-layer ECP stacked film images and Fig.21 As shown in the absorption spectrum in . One of the two-layer ECP stacked films is formed by arranging a cross-linked ECP-Y layer under the top ECP-M layer (FIG. 20(A)), while the other ECP stacked film is formed by arranging a cross-linked ECP-C layer under the top ECP-M layer (FIG. 20(B)). The combination of the ECP-Y and ECP-M layers shows a peach-pink integrated color as shown in FIG. 20(A), and the combination of the ECP-C and ECP-M layers shows a purple-black integrated color as shown in FIG. 20(B). Fig.21 The absorption spectra in further demonstrate that the absorption peak of the bilayer ECP stack film represents the sum of the absorption peaks from its corresponding single-color films. These two example bilayer ECP stack films with different EC layer combinations can show different absorption spectra corresponding to different colors. Figure 20(A) to Figure 20(B) and Fig.21 Both demonstrated that multilayer ECP stack films can form different colors by adjusting the combination of electrochromic materials.

[0071] Film thickness

[0072] Different colors can be achieved by adjusting the thickness of the EC layer. To demonstrate the effect of EC layer thickness on the overall color, two double-layer ECP stack films were made from the same color combination (ECP-Y layer under the top ECP-M layer) with different thicknesses of the individual layers. Since all film casting conditions were the same, there was a correlation between the ECP solution concentration and the film thickness. Figure 11(A) to Figure 11(C) As shown, a higher concentration of ECP solution will produce a thicker EC layer. FIG. 22(A) shows an image of a film having a thicker ECP-Y layer below a thinner top ECP-M layer, while FIG. 22(B) shows an image of a film having a thinner ECP-Y layer below a thicker top ECP-M layer. The film having a thicker ECP-Y layer and a thinner top ECP-M layer ( FIG. 22(A) ) shows a more yellow color than the film having a thinner ECP-Y layer and a thicker top ECP-M layer ( FIG. 22(B) ). Fig.23The absorption spectrum shown also shows less absorption at about 550 nm, but slightly higher absorption at about 450 nm. Figure 22(A) to Figure 22(B) and Fig.23 It was demonstrated that multilayer ECP stacked films can form different colors by adjusting the thickness of each EC layer.

Claims

1. An electrochromic device, characterized in that: include: a first transparent electrode; a plurality of electrochromic layers, which are sequentially stacked on the first transparent electrode, wherein the upper electrochromic layer is arranged on the lower electrochromic layer; an ion storage layer disposed on the electrochromic layer; as well as a second transparent electrode disposed on the ion storage layer, in, The lower electrochromic layer comprises a cross-linked electrochromic layer; and The cross-linked electrochromic layer exhibits solvent resistance to the solvent used in the upper electrochromic layer; Wherein, the electrochromic layer comprises a layer having a cyan electrochromic polymer, a layer having a magenta electrochromic polymer, and a layer having a yellow electrochromic polymer; wherein the electrochromic device exhibits a black color with minimized intermediate colors, in, a film thickness ratio of the layer of the electrochromic polymer having cyan, the layer of the electrochromic polymer having yellow, and the layer of the electrochromic polymer having magenta of 25:8:10; The upper electrochromic layer includes one of the layer having the electrochromic polymer of magenta, the layer having the electrochromic polymer of yellow, and the layer having the electrochromic polymer of cyan, and the lower electrochromic layer includes the other two of the layer having the electrochromic polymer of magenta, the layer having the electrochromic polymer of yellow, and the layer having the electrochromic polymer of cyan.

2. The electrochromic device according to claim 1, characterized in that: The upper electrochromic layer includes the layer of the electrochromic polymer having a magenta color, and the lower electrochromic layer includes the layer of the electrochromic polymer having a cyan color and the layer of the electrochromic polymer having a yellow color, wherein the layer of the electrochromic polymer having a magenta color is a top layer, the layer of the electrochromic polymer having a cyan color is a bottom layer, and the layer of the electrochromic polymer having a yellow color is inserted between the bottom layer and the top layer.

3. The electrochromic device according to claim 2, characterized in that: The uppermost electrochromic layer among the electrochromic layers is cross-linked.

4. The electrochromic device according to claim 2, characterized in that: The crosslinking of the crosslinked electrochromic layer occurs in the absence of a crosslinking agent.

5. The electrochromic device according to claim 2, characterized in that: The crosslinking of the crosslinked electrochromic layer occurs in the presence of a crosslinking agent.

6. The electrochromic device according to claim 2, characterized in that: The film thickness of each of the electrochromic layers is adjusted to obtain different colors.

7. The electrochromic device according to claim 2, characterized in that: The electrochromic layer includes different electrochromic materials to obtain different colors.

8. An electronic device incorporating the electrochromic device according to any one of claims 2 to 7.

9. The electronic device according to claim 8, characterized in that: The electrochromic layer includes a multi-layer electrochromic polymer pattern having surface texture information.

10. A method for controlling the electrochromic or multi-color electrochromic behavior of an electrochromic device according to any one of claims 2 to 7 having a plurality of electrochromic layers, characterized in that: The method includes adjusting the electrochromic material and thickness of each of the electrochromic layers.

Citation Information

Patent Citations

  • Electrochromic display apparatus and method of manufacturing the same

    CN102193263A

  • All-solid-state electrochromic multiple device and preparation method thereof

    CN104423114A

  • Electrochromic device, shell and electronic equipment

    CN110928096A

  • Electrochromic display panel and electronic paper

    CN111123610A

  • Electrochromic display element, display device, information appliance, manufacturing method for electrochromic display element, and electrochromic light control lens

    JP2016156930A