A method for removing impurities from bischlorosulfonyl imide
By using mesoporous molecular sieve adsorbents modified with tantalum and/or niobium, the problem of impurities in the preparation of bischlorosulfonimide by the thionyl chloride method is solved, achieving efficient impurity removal and cost reduction, and ensuring product quality and production safety. .
Patent Information
- Application Number
- CN202310000494.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-01-03
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2043-01-03
AI Technical Summary
There are many heavy component impurities in the existing thionyl chloride method for preparing bischlorosulfonimide, which affects product quality and industrial production safety. Moreover, the existing purification method is cumbersome and costly.
Mesoporous molecular sieves modified by tantalum and/or niobium are used as adsorbents to adsorb heavy tar component impurities such as dichlorodimer and dichlorotrimer in the crude bischlorosulfonimide prepared by the thionyl chloride method. , reduce its content.
It achieves the rapid removal of heavy component impurities such as tar in the crude product without introducing new impurities, significantly improves the impurity removal effect, reduces production costs, and the adsorbent can withstand strong corrosive systems.
Smart Images

Figure GDA0005022256170000111
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of electrolytes, and in particular relates to a method for removing impurities from bischlorosulfonyl imide. Background Art
[0002] At present, electricity is the mainstay of renewable resources. It is an inevitable trend for electric vehicles to replace oil vehicles. With the increasing maturity of lithium battery technology, the popularity of electric vehicles has been further pushed to a climax. The demand for batteries has increased sharply, especially the demand for lithium batteries, which is in short supply, and the price of the electrolytes they match has also risen. Whether a battery can have excellent performance is not only dominated by the design and electrodes, but also by the performance of the electrolyte. Therefore, the research work on electrolytes is a long and arduous task.
[0003] Nowadays, lithium batteries occupy a dominant position in the battery industry. There are endless methods for preparing various electrolytes. The synthesis of lithium hexafluorophosphate and lithium bis(fluorosulfonyl)imide is in full swing. Among them, lithium bis(fluorosulfonyl)imide, as an electrolyte additive, is increasingly recognized by the market due to its excellent product performance, and the market demand is increasing day by day.
[0004] In the existing synthesis of lithium bis(fluorosulfonyl)imide, the more commonly used routes are the thionyl chloride method and the isocyanate method:
[0005] Isocyanate method: Although there are fewer side reactions, fewer impurities, and the post-processing is relatively simple, the raw materials are expensive and it is difficult to maintain competitiveness in the market.
[0006] Sulfonyl chloride method: The raw material price is low and the reaction difficulty is relatively small. It is accepted by more and more people and gradually becomes the mainstream production route in the industry. In the thionyl chloride synthesis route, bis(chlorosulfonyl)imide is an extremely important intermediate product, and its product index directly affects the operation of subsequent reaction steps and the quality of the final product. However, during the chlorination reaction, due to the long reaction time, relatively high temperature, and more side reactions, more heavy component impurities will be generated. These impurities not only affect the subsequent reaction and product quality, but also have great safety hazards for industrial production.
[0007] Patent CN115304039A provides a method for purifying bischlorosulfonyl imide, which uses a melt crystallizer and a falling film evaporator to remove heavy component impurities of bischlorosulfonyl imide. Although this method can purify the purity to 99.5%, the operation process is cumbersome and there are still many impurities in the final product.
[0008] Therefore, in the art, for this mainstream route, it is desired to develop an economical and efficient method to reduce the content of heavy component impurities in the bischlorosulfonimide product. Summary of the invention
[0009] In view of the above problems existing in the prior art, the present invention aims to provide a method for removing impurities from bischlorosulfonyl imide. The present invention uses a mesoporous molecular sieve modified with tantalum or niobium as an adsorbent, which can quickly adsorb tar heavy component impurities such as dichloro dimer and dichloro trimer in the crude bischlorosulfonyl imide prepared by the thionyl chloride method.
[0010] The invention provides a method for removing impurities from bischlorosulfonyl imide. The method uses a mesoporous molecular sieve modified with metal tantalum and / or niobium as an adsorbent to adsorb impurities in a crude bischlorosulfonyl imide product prepared by a thionyl chloride method.
[0011] In the impurity removal method of the present invention, the crude bischlorosulfonyl imide obtained by the thionyl chloride method comprises 10-99.5% by weight of bischlorosulfonyl imide, preferably 95-99.5% by weight; 0-60% by weight of thionyl chloride, preferably 0-40% by weight; 0-5% by weight of chlorosulfonic acid, preferably 0-2% by weight; 0-5% by weight of aminosulfonic acid, preferably 0-3% by weight; and 0.5-10% by weight of impurities, preferably 0.5-5%; wherein the impurities include tar heavy components such as dichloro dimer and dichloro trimer.
[0012] The crude bis(fluorosulfonyl)imide obtained by the thionyl chloride method is a prior art, and the present invention does not limit its specific preparation process. The crude bis(chlorosulfonyl)imide can be a reaction solution obtained by direct reaction of thionyl chloride, chlorosulfonic acid, and aminosulfonic acid, or a sub-pure product after rectification treatment to remove unreacted raw materials such as thionyl chloride, chlorosulfonic acid, and aminosulfonic acid. As long as the material is prepared by the thionyl chloride method and is within the concentration range, it belongs to the crude product suitable for the impurity removal method of the present invention. The crude product can be liquid or solid. When the crude product is solid, it can be melted into a liquid state at the adsorption temperature and subjected to adsorption and impurity removal treatment.
[0013] In the impurity removal method of the present invention, the mesoporous molecular sieve modified with metal tantalum and / or niobium, wherein the content of metal tantalum and / or niobium is 0.5-20wt%, preferably 5-16wt%;
[0014] Preferably, the mesoporous molecular sieve has a pore size of 2-11 nm, more preferably SBA-15 and / or MCM-41;
[0015] More preferably, the metal tantalum and / or niobium modified mesoporous molecular sieve is selected from tantalum-modified SBA-15 and / or niobium-modified MCM-41;
[0016] The mesoporous molecular sieve modified with metal tantalum and / or niobium can be prepared by conventional methods disclosed in the prior art, such as impregnation method, and the present invention does not specifically limit it. In some specific examples of the present invention, the mesoporous molecular sieve modified with metal tantalum and / or niobium can be prepared by the following method, comprising the steps of:
[0017] 1) adding the mesoporous molecular sieve into a sodium hydroxide aqueous solution for immersion and elution, then washing with water until neutral, and drying to constant weight;
[0018] 2) placing the mesoporous molecular sieve treated in step 1) in an aqueous solution of a soluble salt of metal tantalum and / or niobium, stirring the solution sufficiently, and then adjusting the pH value to 9-11 with aqueous ammonia;
[0019] 3) The system of step 2) is filtered and dried by spin drying, then calcined in an air environment, and then calcined in a hydrogen-nitrogen mixed gas to obtain the metal tantalum and / or niobium modified mesoporous molecular sieve.
[0020] Preferably, in step 1), the concentration of the sodium hydroxide aqueous solution is 0.5-2 mol / L, preferably 1-1.5 mol / L.
[0021] Preferably, in step 1), the immersion and elution time is 1-12 hours, preferably 4-8 hours.
[0022] Preferably, in step 2), the aqueous solution of soluble salts of metal tantalum and / or niobium, wherein the total concentration of soluble salts of tantalum and soluble salts of niobium is 1-20wt%, preferably 5-16wt%;
[0023] More preferably, the soluble salt is a hydrochloride or a fluoride salt, such as tantalum pentafluoride or niobium chloride.
[0024] Preferably, in step 2), the stirring is performed sufficiently at a temperature of 40-70°C, preferably 45-60°C, for a time of 10-60 min, preferably 30-50 min.
[0025] Preferably, in step 2), the concentration of the aqueous ammonia is 10-25wt%, preferably 15-20wt%; and the system temperature during the pH adjustment process is 40-70°C, preferably 50-60°C.
[0026] Preferably, in step 3), the calcination temperature is 400-700° C., preferably 500-600° C., and the time is 1-12 h, preferably 6-10 h.
[0027] Preferably, in step 3), the calcination temperature is 400-600° C., preferably 400-500° C., and the time is 1-10 h, preferably 4-8 h;
[0028] The hydrogen-nitrogen mixed gas contains 0.5-5wt% hydrogen, preferably 2-4wt%.
[0029] The above-mentioned method for preparing the mesoporous molecular sieve modified with metal tantalum and / or niobium also includes conventional operations in the art such as water washing, drying, spin drying, filtering, etc., which are not particularly required by the present invention.
[0030] The mesoporous molecular sieve modified with metal tantalum and / or niobium of the present invention is prepared by first pre-treating and eluting the mesoporous molecular sieve with a sodium hydroxide aqueous solution of appropriate concentration, and then introducing an appropriate amount of metal tantalum and / or niobium to fill it, which can not only completely replace the original aluminum atoms to construct a new metal framework, but also etch new channels; the metal framework newly constructed by the method of the present invention has a more stable structure, and then new channels are formed by appropriate replacement methods, dispersion methods, etching, and calcination temperatures, and the modified mesoporous molecular sieve thus prepared has a better adsorption effect on heavy component tar macromolecular impurities such as dichloro dimer and dichloro trimer in the system; at the same time, the modified metal tantalum and / or niobium introduced by the present invention can not only perform complex adsorption with the heavy components in the raw material to improve the adsorption efficiency, but also form more stable new bonds with the silicon-oxygen atoms in the molecular sieve, so that the adsorbent maintains a long service life in the strong corrosion system.
[0031] In the impurity removal method of the present invention, the adsorption temperature is 30-100°C, preferably 40-70°C, the pressure is 0.1-5MPaG, preferably 0.3-3MPaG; the adsorption residence time is 70-720s, preferably 180-360s;
[0032] The mass space velocity during the adsorption process is 5-50h -1 , preferably 10-20h -1 .
[0033] Preferably, the adsorption is performed in a nitrogen environment.
[0034] The adsorption process is carried out in an adsorption device. The type of the adsorption device has little effect on the impurity removal effect. It can be a fixed bed, a reactor, etc., and the present invention does not make specific limitations.
[0035] During the adsorption process, the required adsorption raw materials enter the heated premixing zone. After being premixed to the specified temperature in the premixing zone, the pre-adsorption raw materials are pumped through the adsorbent filling zone at a preset flow rate through the feed pump. The adsorbent filling zone maintains the adsorption temperature through heating, and the adsorption pressure through inert gas. The qualified products in the discharging zone are taken out through the discharging pump.
[0036] The content of heavy component tar impurities such as dichloro dimer and dichloro trimer in the impurity-removed product obtained by the impurity-removing method of the present invention can be reduced to below 0.05% based on the mass after deducting unreacted raw materials such as thionyl chloride, chlorosulfonic acid, and aminosulfonic acid.
[0037] Compared with the prior art, the technical solution of the present invention has the following beneficial effects:
[0038] The method of the present invention can quickly remove heavy component impurities such as tar in the crude raw material without introducing new impurities, thereby achieving early impurity removal without the need to continue to bring impurities into subsequent applications. The impurity removal effect is significant, the production cost is low, and the adsorbent can well tolerate the strong corrosion system of the raw material. DETAILED DESCRIPTION
[0039] In order to better understand the technical solution of the present invention, the content of the present invention is further described below in conjunction with the embodiments, but the content of the present invention is not limited to the following embodiments.
[0040] The main sources of raw materials used in the examples of the present invention are as follows. Other raw materials are common commercially available unless otherwise specified:
[0041] Mesoporous molecular sieve SBA-15, pore size 3.5-10nm, brand: INNOCHEM, item number: SBA-15;
[0042] Mesoporous molecular sieve MCM-41 molecular sieve, pore size 2-8nm, brand: Clamart, item number: 105120;
[0043] Tantalum fluoride, brand: ALFA, product number: 014052, purity: 99.9%;
[0044] Niobium pentachloride, brand: innochem, product number: A81205, purity: 99.9%;
[0045] Preparation process of crude bis(chlorosulfonyl)imide by thionyl chloride method: thionyl chloride, aminosulfonic acid and chlorosulfonic acid are reacted at a suitable temperature according to a certain ratio to obtain the crude product; the crude product is a sub-pure product after solvent removal through distillation purification, or a bottom liquid doped with heavy components that stays for a long time during the distillation process.
[0046] Unless otherwise specified, the experimental operations involved in the following examples or comparative examples are all conventional experimental methods in the art.
[0047] Analytical method: NMR instrument: Bruker AVANCE III 400M configuration: ULTRASHIELD 400 magnet / B-ACS 60-position autosampler / Topstin 3.0 software / 5mm Dual (13C, 1H) dual nuclear probe / 5mm BBO probe.
[0048] Example 1
[0049] Tantalum-modified SBA-15 molecular sieve (adsorbent 1), the steps are:
[0050] 1) Add the SBA-15 molecular sieve into a 1.2 mol / L sodium hydroxide aqueous solution for immersion and elution for 7 hours, then rinse with ultrapure water until neutral, and dry at 120°C to constant weight;
[0051] 2) The SBA-15 molecular sieve treated in step 1) is placed in a 16wt% tantalum fluoride aqueous solution, and stirred at 50°C for 45min. Then, under this condition, 18wt% ammonia water is added dropwise to adjust the pH to 9-11. The mixture is then spin-dried and filtered. After being dried to constant weight at 120°C, it is calcined at 550°C for 9h. A hydrogen-nitrogen mixed gas with a hydrogen content of 3.5wt% is then introduced, and calcined at 490°C for 8h to obtain tantalum-modified SBA-15 with a tantalum content of 11wt%.
[0052] Example 2
[0053] The niobium-modified MCM-41 molecular sieve (adsorbent 2) was prepared by:
[0054] 1) Add the MCM-41 molecular sieve into a 2 mol / L sodium hydroxide aqueous solution for immersion and elution for 1 hour, then rinse with ultrapure water until neutral, and dry at 100°C to constant weight;
[0055] 2) The MCM-41 molecular sieve treated in step 1) is placed in a 5wt% niobium chloride aqueous solution, and stirred at 40°C for 60 minutes. Then, under the same condition, 10wt% ammonia water is added dropwise to adjust the pH to 9-11. The mixture is then spin-dried and filtered. After being dried to constant weight at 100°C, it is calcined at 700°C for 1h. A hydrogen-nitrogen mixed gas with a hydrogen content of 0.5wt% is then introduced, and calcined at 400°C for 4h to obtain niobium-modified ZSM-5 with a niobium content of 4.0wt%.
[0056] Example 3
[0057] Tantalum-modified MCM-41 molecular sieve (adsorbent 3) was prepared by the following steps:
[0058] 1) Add the MCM-41 molecular sieve into a 0.5 mol / L sodium hydroxide aqueous solution for immersion and elution for 12 h, then rinse with ultrapure water until neutral, and dry at 130° C. to constant weight;
[0059] 2) The MCM-41 molecular sieve treated in step 1) is placed in a 20wt% tantalum pentachloride aqueous solution, and stirred at 40°C for 60 minutes. Then, under the same condition, 25wt% ammonia water is added dropwise to adjust the pH to 9-11. The mixture is then spin-dried and filtered. After being dried to constant weight at 100°C, the mixture is calcined at 400°C for 10 hours. A hydrogen-nitrogen mixed gas with a hydrogen content of 0.5wt% is then introduced, and the mixture is calcined at 500°C for 10 hours to obtain niobium-modified MCM-41 with a tantalum content of 12.5wt%.
[0060] Example 4
[0061] The niobium-modified SBA-15 molecular sieve (adsorbent 4) was prepared by:
[0062] 1) Add the SBA-15 molecular sieve into a 1.5 mol / L sodium hydroxide aqueous solution for immersion and elution for 6 hours, then rinse with ultrapure water until neutral, and dry at 100°C to constant weight;
[0063] 2) The SBA-15 molecular sieve treated in step 1) is placed in a 3wt% niobium chloride aqueous solution, and stirred at 40°C for 60 minutes. Then, under the same condition, 20wt% ammonia water is added dropwise to adjust the pH to 9-11. The mixture is then spin-dried and filtered. After being dried to constant weight at 100°C, the mixture is calcined at 700°C for 1h. A hydrogen-nitrogen mixed gas with a hydrogen content of 0.5wt% is then introduced, and the mixture is calcined at 550°C for 4h to obtain niobium-modified SBA-15 with a niobium content of 2.5wt%.
[0064] Example 5
[0065] The crude product of bischlorosulfonyl imide (sub-pure product after distillation) has the following mass percentage compositions: 97.5wt% of bischlorosulfonyl imide and 2.5wt% of impurities (including bischloro dimer and bischloro trimer).
[0066] The steps of removing impurities with bis(chlorosulfonyl)imide are as follows:
[0067] The crude product was preheated to 50°C and then pumped into the adsorption device using a feed pump. Nitrogen was introduced at the same time to control the pressure to 2 MPaG and the temperature to 60°C. The product was then passed through the adsorption zones of the adsorbents 1-4 prepared in Examples 1-4 for adsorption and impurity removal at a space velocity of 15 h -1 , adsorption residence time 240S, after the device is running stably, samples are taken from the product discharge area to detect the impurity content in the product. The results are shown in Table 1.
[0068] After 100 h of continuous operation, the adsorption performance decay rate and dissolution rate were tested. The results are shown in Table 1.
[0069] Table 1
[0070] Adsorbent Impurity content / % Adsorption performance decay rate after 100h / % Dissolution rate after 100h / % Adsorbent 1 0.01 1 0.1 Adsorbent 2 0.04 2 0.15 Adsorbent 3 0.03 1.5 0.15 Adsorbent 4 0.05 1.8 0.1
[0071] Example 6
[0072] The crude product of bischlorosulfonyl imide (reaction solution) has the following mass percentage composition: bischlorosulfonyl imide 89wt%, thionyl chloride 8.5wt%; chlorosulfonic acid 0.5wt%, aminosulfonic acid 0.5wt%; impurities (including bischloro dimer and bischloro trimer) 1.5wt%;
[0073] The crude product was preheated to 50°C and then pumped into the adsorption device using a feed pump. Nitrogen was introduced at the same time to control the pressure to 2 MPaG and the temperature to 60°C. The product was then passed through the adsorption zones of the adsorbents 1-4 prepared in Examples 1-4 for adsorption and impurity removal at a space velocity of 15 h -1 , adsorption residence time 240S, after the device is running stably, samples are taken from the product discharge area to detect the impurity content in the product (calculated based on the mass after deducting unreacted raw materials such as thionyl chloride, chlorosulfonic acid, and aminosulfonic acid). The results are shown in Table 2.
[0074] After 100 h of continuous operation, the adsorption performance decay rate and dissolution rate were tested. The results are shown in Table 2.
[0075] Table 2
[0076] Adsorbent Impurity content / % Adsorption performance decay rate after 100h / % Dissolution rate after 100h / % Adsorbent 1 0.01 1 0.1 Adsorbent 2 0.02 1.5 0.1 Adsorbent 3 0.01 1 0.1 Adsorbent 4 0.04 1.3 0.1
[0077] Example 7
[0078] The crude product of bischlorosulfonyl imide (sub-pure product after distillation) has the following mass percentage compositions: 99.5wt% of bischlorosulfonyl imide and 0.5wt% of impurities (including bischloro dimer and bischloro trimer).
[0079] The steps of removing impurities with bis(chlorosulfonyl)imide are as follows:
[0080] The crude product was preheated to 30°C and then pumped into the adsorption device using a feed pump. Nitrogen was introduced at the same time to control the pressure to 0.1 MPaG and the temperature to 30°C. The product was then passed through the adsorption zones of the adsorbents 1-4 prepared in Examples 1-4 for adsorption and impurity removal at a space velocity of 50 h -1 , adsorption residence time 72S, after the device is running stably, samples are taken from the product discharge area to detect the impurity content in the product. The results are shown in Table 3.
[0081] After running continuously for 100 h, the adsorption performance decay rate and dissolution rate were tested. The results are shown in Table 3.
[0082] Table 3
[0083] Adsorbent Impurity content / % Adsorption performance decay rate after 100h / % Dissolution rate after 100h / % Adsorbent 1 0.01 1.5 0.15 Adsorbent 2 0.02 1.9 0.18 Adsorbent 3 0.01 1.5 0.13 Adsorbent 4 0.03 1.8 0.12
[0084] Example 8
[0085] The crude product of bischlorosulfonyl imide (reaction solution) has the following mass percentage compositions: bischlorosulfonyl imide 15wt%, thionyl chloride 83wt%; chlorosulfonic acid 0.7wt%, aminosulfonic acid 0.8wt%; impurities (including bischloro dimer and bischloro trimer) 0.5wt%;
[0086] The crude product was preheated to 30°C and pumped into the adsorption device using a feed pump. Nitrogen was introduced at the same time to control the pressure to 5 MPaG and the temperature to 30°C. The product was then passed through the adsorption zones of the adsorbents 1-4 prepared in Examples 1-4 for adsorption and impurity removal at a space velocity of 15 h -1 , adsorption residence time 240S, after the device is running stably, samples are taken from the product discharge area to detect the impurity content in the product (the mass after deducting unreacted raw materials such as thionyl chloride, chlorosulfonic acid, and aminosulfonic acid is used as the basis for calculation), and the results are shown in Table 4.
[0087] After 100 h of continuous operation, the adsorption performance decay rate and dissolution rate were tested. The results are shown in Table 4.
[0088] Table 4
[0089]
[0090]
[0091] Example 9
[0092] The crude product of bischlorosulfonyl imide (sub-pure product after distillation) has the following mass percentage compositions: 95.5 wt % of bischlorosulfonyl imide and 4.5 wt % of impurities (including bischloro dimer and bischloro trimer).
[0093] The steps of removing impurities with bis(chlorosulfonyl)imide are as follows:
[0094] The crude product was preheated to 60°C and then pumped into the adsorption device using a feed pump. Nitrogen was introduced to control the pressure to 3 MPa and the temperature to 70°C. The adsorption and impurity removal was carried out by the adsorption zone of the adsorbent 1-4 prepared in Example 1-4 at a space velocity of 5 h -1 , adsorption residence time 720S, after the device is running stably, samples are taken from the product discharge area to detect the impurity content in the product. The results are shown in Table 5.
[0095] After 100 h of continuous operation, the adsorption performance decay rate and dissolution rate were tested. The results are shown in Table 5.
[0096] Table 5
[0097] Adsorbent Impurity content / % Adsorption performance decay rate after 100h / % Dissolution rate after 100h / % Adsorbent 1 0.01 1.1 0.1 Adsorbent 2 0.02 1.2 0.15 Adsorbent 3 0.01 1.5 0.15 Adsorbent 4 0.03 1.8 0.1
[0098] Example 10
[0099] The crude product of bischlorosulfonyl imide (reaction solution) has the following mass percentage compositions: bischlorosulfonyl imide 35wt%, thionyl chloride 59wt%; chlorosulfonic acid 1.1wt%, aminosulfonic acid 1.4wt%; impurities (including bischloro dimer and bischloro trimer) 3.5wt%;
[0100] The crude product was preheated to 60°C and then pumped into the adsorption device using a feed pump. Nitrogen was introduced at the same time to control the pressure to 5 MPaG and the temperature to 70°C. The product was then passed through the adsorption zones of the adsorbents 1-4 prepared in Examples 1-4 for adsorption and impurity removal at a space velocity of 15 h -1 , adsorption residence time 240S, after the device is running stably, samples are taken from the product discharge area to detect the impurity content in the product (the mass after deducting unreacted raw materials such as thionyl chloride, chlorosulfonic acid, and aminosulfonic acid is used as the basis for calculation), and the results are shown in Table 6.
[0101] After 100 h of continuous operation, the adsorption performance decay rate and dissolution rate were tested. The results are shown in Table 6.
[0102] Table 6
[0103] Adsorbent Impurity content / % Adsorption performance decay rate after 100h / % Dissolution rate after 100h / % Adsorbent 1 0.01 1.2 0.1 Adsorbent 2 0.04 1.1 0.15 Adsorbent 3 0.03 1.3 0.1 Adsorbent 4 0.05 1.2 0.1
[0104] Comparative Example 1
[0105] The adsorbent was prepared by referring to the method of Example 1, except that the SBA-15 mesoporous molecular sieve was replaced by 5A molecular sieve, and other operations remained unchanged, thereby obtaining tantalum-modified 5A molecular sieve.
[0106] The impurity removal of the sub-pure product of bis(chlorosulfonyl)imide was carried out according to the method of Example 5, except that the adsorbent was replaced with the prepared tantalum-modified 5A molecular sieve adsorbent, and other operations and conditions remained unchanged. The impurity content in the product after treatment was 2.1 wt %; after continuous operation for 100 h, the adsorption performance attenuation rate was 60.5%, and the dissolution loss rate was 2.5%.
[0107] The bischlorosulfonyl imide reaction solution was impurity-removed by referring to the method of Example 6, except that the adsorbent was replaced with the prepared tantalum-modified 5A molecular sieve adsorbent, and other operations and conditions remained unchanged. The impurity content in the product after treatment was 1.5wt%; after continuous operation for 100h, the adsorption performance attenuation rate was 30.6%, and the dissolution loss rate was 2.2%.
[0108] Comparative Example 2
[0109] The adsorbent was prepared by referring to the method of Example 1, except that the SBA-15 mesoporous molecular sieve was replaced by 4A molecular sieve, and other operations remained unchanged, thereby obtaining tantalum-modified 4A molecular sieve.
[0110] The impurity content of the sub-pure product of bis(chlorosulfonyl)imide was removed by referring to the method of Example 5, and the adsorbent was replaced by the prepared tantalum-modified 4A molecular sieve adsorbent. Other operations and conditions remained unchanged. The impurity content in the product after treatment was 2.45wt%; after continuous operation for 100h, the adsorption performance decay rate was 27.6%, and the dissolution loss rate was 1.9%.
[0111] The bischlorosulfonyl imide reaction solution was impurity-removed by referring to the method of Example 6, except that the adsorbent was replaced with the prepared tantalum-modified 4A molecular sieve adsorbent, and other operations and conditions remained unchanged. The impurity content in the product after treatment was 1.56wt%; after continuous operation for 100h, the adsorption performance attenuation rate was 28.4%, and the dissolution loss rate was 2.2%.
[0112] Comparative Example 3
[0113] The adsorbent was prepared by referring to the method of Example 1, except that the SBA-15 mesoporous molecular sieve was replaced by a microporous molecular sieve ZSM-5 with a pore size of about 0.55 nm, and other operations remained unchanged, thereby obtaining a tantalum-modified ZSM-5 molecular sieve.
[0114] The impurity removal of the sub-pure product of bis(chlorosulfonyl)imide was carried out according to the method of Example 5, and the adsorbent was replaced by the prepared tantalum-modified adsorbent. Other operations and conditions remained unchanged. The impurity content in the product after treatment was 2.3wt%. After continuous operation for 100h, the adsorption performance decay rate was 15%, and the dissolution loss rate was 1.0%.
[0115] The bischlorosulfonyl imide reaction solution was impurity-removed by referring to the method of Example 6, except that the adsorbent was replaced with the prepared tantalum-modified ZSM-5 adsorbent, and other operations and conditions remained unchanged. The impurity content in the product after treatment was 1.61wt%; after continuous operation for 100h, the adsorption performance attenuation rate was 21.2%, and the dissolution loss rate was 2.1%.
[0116] Comparative Example 4
[0117] The adsorbent was prepared by referring to the method of Example 1, except that the modified metal tantalum was replaced by vanadium, and other operations remained unchanged, thereby obtaining a vanadium-modified SBA-15 molecular sieve.
[0118] The impurity removal of the sub-pure bischlorosulfonyl imide was carried out according to the method of Example 5, and the adsorbent was replaced by the prepared vanadium-modified SBA-15 molecular sieve adsorbent. Other operations and conditions remained unchanged. The impurity content in the product after treatment was 2.2wt%; after continuous operation for 100h, the adsorption performance decay rate was 36%, and the dissolution loss rate was 0.5%.
[0119] The bischlorosulfonyl imide reaction solution was impurity-removed by referring to the method of Example 6, except that the adsorbent was replaced with the prepared vanadium-modified SBA-15 molecular sieve adsorbent, and other operations and conditions remained unchanged. The impurity content in the product after treatment was 1.9wt%; after continuous operation for 100h, the adsorption performance attenuation rate was 33.4%, and the dissolution loss rate was 0.4%.
[0120] Comparative Example 5
[0121] The adsorbent was prepared by referring to the method of Example 1, except that the modified metal tantalum was replaced by molybdenum, and other operations remained unchanged, thereby obtaining a molybdenum-modified SBA-15 molecular sieve.
[0122] The impurity removal of the sub-pure product of bischlorosulfonyl imide was carried out according to the method of Example 5, and the adsorbent was replaced by the prepared molybdenum-modified SBA-15 molecular sieve adsorbent. Other operations and conditions remained unchanged. The impurity content in the product after treatment was 2.4wt%; after continuous operation for 100h, the adsorption performance attenuation rate was 20.6%, and the dissolution loss rate was 0.4%.
[0123] The bischlorosulfonyl imide reaction solution was impurity-removed by referring to the method of Example 6, except that the adsorbent was replaced with the prepared molybdenum-modified SBA-15 molecular sieve adsorbent, and other operations and conditions remained unchanged. The impurity content in the treated product was 1.46wt%; after continuous operation for 100h, the adsorption performance attenuation rate was 29.2.1%, and the dissolution loss rate was 0.6%.
[0124] Comparative Example 6
[0125] The method of Example 5 is used to remove impurities from the sub-pure product of bis(chlorosulfonyl)imide. The only difference is that: unmodified SBA-15 is directly used as the adsorbent, and other operations and conditions remain unchanged. The impurity content in the product after treatment is 2.4wt%; after continuous operation for 100h, the adsorption performance decay rate is 19.6%, and the dissolution loss rate is 0.1%.
[0126] The impurity removal of the bis(chlorosulfonyl)imide reaction solution was carried out according to the method of Example 6, except that unmodified SBA-15 was directly used as the adsorbent, and other operations and conditions remained unchanged. The impurity content in the product after treatment was 1.57 wt %; after continuous operation for 100 h, the adsorption performance attenuation rate was 20.7%, and the dissolution loss rate was 0.1%.
[0127] Comparative Example 7
[0128] The method of Example 5 is used to remove impurities from the semi-pure product of bischlorosulfonyl imide, the only difference being that unmodified MCM-41 is directly used as the adsorbent, and other operations and conditions remain unchanged. The impurity content in the semi-pure product after treatment is 2.3wt%; after continuous operation for 100h, the adsorption performance decay rate is 24.5%, and the dissolution loss rate is 0.1%.
[0129] The bischlorosulfonyl imide reaction solution was impurity-removed by referring to the method of Example 6, except that: unmodified MCM-41 was directly used as the adsorbent, and other operations and conditions remained unchanged. The impurity content in the treated product was 1.41wt%; after continuous operation for 100h, the adsorption performance attenuation rate was 23.7%, and the dissolution loss rate was 0.1%.
[0130] Comparative Example 8
[0131] The adsorbent was prepared by referring to the method of Example 1, except that the preparation process did not use step 1) alkaline impregnation and elution, and other operations remained unchanged to obtain a tantalum-modified SBA-15 molecular sieve.
[0132] The impurity removal of the sub-pure product of bis(chlorosulfonyl)imide was carried out according to the method of Example 5, and the adsorbent was replaced by the prepared tantalum-modified SBA-15 molecular sieve adsorbent. Other operations and conditions remained unchanged. The impurity content in the product after treatment was 2.35wt%. After continuous operation for 100h, the adsorption performance decay rate was 32.7%, and the dissolution loss rate was 1.5%.
[0133] The bischlorosulfonyl imide reaction solution was deimpregnated by referring to the method of Example 6, and the adsorbent was replaced by the prepared tantalum-modified SBA-15 molecular sieve molecular sieve adsorbent. Other operations and conditions remained unchanged. The impurity content in the product after treatment was 1.55wt%; after continuous operation for 100h, the adsorption performance attenuation rate was 29.3%, and the dissolution loss rate was 1.7%.
[0134] Comparative Example 9
[0135] The adsorbent was prepared by referring to the method of Example 1, except that there was no calcination operation in step 2) of the preparation process, and other operations remained unchanged, thereby obtaining a tantalum-modified SBA-15 molecular sieve.
[0136] The impurity removal of the sub-pure product of bis(chlorosulfonyl)imide was carried out according to the method of Example 5, and the adsorbent was replaced by the prepared tantalum-modified SBA-15 molecular sieve adsorbent. Other operations and conditions remained unchanged. The impurity content in the product after treatment was 1.2 wt %. After continuous operation for 100 h, the adsorption performance attenuation rate was 5.4%, and the dissolution loss rate was 1.7%.
[0137] The bischlorosulfonyl imide reaction solution was impurity-removed by referring to the method of Example 6, and the adsorbent was replaced by the prepared tantalum-modified SBA-15 molecular sieve molecular sieve adsorbent. Other operations and conditions remained unchanged. The impurity content in the product after treatment was 1.1wt%; after continuous operation for 100h, the adsorption performance attenuation rate was 7.6%, and the dissolution loss rate was 1.3%.
[0138] Those skilled in the art will appreciate that, based on the teachings of this specification, some modifications or adjustments may be made to the present invention, and these modifications or adjustments should also be within the scope defined by the claims of the present invention.
Claims
1. A method for removing impurities from bischlorosulfonyl imide, characterized in that: The method uses a mesoporous molecular sieve modified with metal tantalum and / or niobium as an adsorbent to adsorb impurities in a crude bischlorosulfonyl imide product prepared by a thionyl chloride method; The mesoporous molecular sieve modified with metal tantalum and / or niobium, wherein the content of metal tantalum and / or niobium is 0.5-20wt%; The mesoporous molecular sieve modified with metal tantalum and / or niobium is prepared by the following method, which comprises the following steps: 1) adding the mesoporous molecular sieve into a sodium hydroxide aqueous solution for immersion and elution, then washing with water until neutral, and drying to constant weight; 2) placing the mesoporous molecular sieve treated in step 1) in an aqueous solution of a soluble salt of metal tantalum and / or niobium, stirring the solution sufficiently, and then adjusting the pH value to 9-11 with aqueous ammonia; 3) The system of step 2) is filtered and dried by spin drying, then calcined in an air environment, and then calcined in a hydrogen-nitrogen mixed gas to obtain the metal tantalum and / or niobium modified mesoporous molecular sieve.
2. The impurity removal method according to claim 1, characterized in that: The crude bischlorosulfonyl imide obtained by the thionyl chloride method comprises 10-99.5wt% of bischlorosulfonyl imide, 0-60wt% of thionyl chloride, 0-5wt% of chlorosulfonic acid, 0-5wt% of aminosulfonic acid and 0.5-10wt% of impurities in terms of weight percentage.
3. The impurity removal method according to claim 2, characterized in that: The crude bischlorosulfonyl imide obtained by the thionyl chloride method comprises 95-99.5wt% of bischlorosulfonyl imide, 0-40wt% of thionyl chloride, 0-2wt% of chlorosulfonic acid, 0-3wt% of aminosulfonic acid and 0.5-5wt% of impurities in terms of weight percentage.
4. The impurity removal method according to claim 1, characterized in that: The content of the metal tantalum and / or niobium is 5-16wt%.
5. The impurity removal method according to claim 1, characterized in that: The pore size of the mesoporous molecular sieve is 2-11 nm.
6. The impurity removal method according to claim 1, characterized in that: The mesoporous molecular sieve is SBA-15 and / or MCM-41.
7. The impurity removal method according to claim 1, characterized in that: The tantalum and / or niobium modified mesoporous molecular sieve is selected from tantalum modified SBA-15 and / or niobium modified MCM-41.
8. The impurity removal method according to claim 1, characterized in that: In step 1), the concentration of the sodium hydroxide aqueous solution is 0.5-2 mol / L; In step 1), the immersion and elution time is 1-12 hours.
9. The impurity removal method according to claim 8, characterized in that: The concentration of the sodium hydroxide aqueous solution is 1-1.5 mol / L.
10. The impurity removal method according to claim 8, characterized in that: The immersion and elution time is 4-8h.
11. The impurity removal method according to claim 1, characterized in that: In step 2), the aqueous solution of soluble salts of metal tantalum and / or niobium, wherein the total concentration of soluble salts of tantalum and soluble salts of niobium is 1-20wt%; In step 2), the stirring is sufficient at a temperature of 40-70° C. for 10-60 min; In step 2), the concentration of the aqueous ammonia is 10-25 wt %; the system temperature during the pH adjustment process is 40-70° C.
12. The impurity removal method according to claim 11, characterized in that: The aqueous solution of soluble salts of metal tantalum and / or niobium, wherein the total concentration of the soluble salts of tantalum and niobium is 5-16 wt %.
13. The impurity removal method according to claim 11, characterized in that: The sufficient stirring is performed at a temperature of 45-60°C and a time of 30-50 minutes.
14. The impurity removal method according to claim 11, characterized in that: The concentration of the ammonia water is 15-20 wt %; the system temperature during the pH adjustment process is 50-60° C.
15. The impurity removal method according to claim 1, characterized in that: In step 2), the soluble salt is hydrochloride or fluoride salt.
16. The impurity removal method according to claim 1, characterized in that: In step 3), the calcination temperature is 400-700°C and the time is 1-12h; In step 3), the calcination temperature is 400-600°C and the time is 1-10h; The hydrogen-nitrogen mixed gas contains 0.5-5wt% hydrogen.
17. The impurity removal method according to claim 16, characterized in that: The calcination temperature is 500-600°C and the time is 6-10h.
18. The impurity removal method according to claim 16, characterized in that: The calcination temperature is 400-500° C. and the calcination time is 4-8 hours.
19. The impurity removal method according to claim 16, characterized in that: The hydrogen-nitrogen mixed gas contains 2-4 wt% hydrogen.
20. The impurity removal method according to claim 1, characterized in that: The adsorption temperature is 30-100° C., the pressure is 0.1-5 MPaG, and the adsorption residence time is 70-720 s.
21. The impurity removal method according to claim 20, characterized in that: The adsorption temperature is 40-70°C, the pressure is 0.3-3MPaG, and the adsorption residence time is 180-360s.
22. The impurity removal method according to claim 1, characterized in that: The adsorption was carried out in a nitrogen environment.
23. The impurity removal method according to claim 1, characterized in that: The mass space velocity during the adsorption process is 5-50h -1 .
24. The impurity removal method according to claim 23, characterized in that: The mass space velocity during the adsorption process is 10-20h -1 .
Citation Information
Patent Citations
Preparation method and preparation equipment of high-purity bis (chlorosulfonyl) imide
CN115215306A
Device and method for purifying bis (chlorosulfonyl) imide
CN115304039A