Method for forming silicone layer on surface of metal part and silicone layer

The silicone layer on the surface of the metal parts is formed by spraying AB mixture with components such as vinyl silicone oil, which solves the problems of insolidity and low production efficiency in the prior art, and achieves a high-strength, durable and beautiful silicone layer. Improves user experience and service life.

CN116478619BActive Publication Date: 2024-11-12FOSHAN SHUNDE DISTRICT KANGXI RUBBER GLUE IND TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210045515.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-01-15
Publication Date
2024-11-12
Estimated Expiration
2042-01-15

AI Technical Summary

Technical Problem

The existing metal parts package silicone structure has low production efficiency, the silicone layer is not firm and easy to fall off, resulting in poor texture and non-heat insulation.

Method used

AB mixture of components such as vinyl silicone oil, platinum water, silane coupling agent, vapor-phase white carbon black and aluminum hydroxide is used to form a silicone layer through the spraying process, and a locking buckle is formed by baking and multiple spraying intervals. Structure, improve adhesion and strength.

Benefits of technology

It achieves efficient molding of the silicone layer, with tensile strength greater than 6MPA, tear strength greater than 20N/MM, and is not easy to fall off, improving the texture and thermal insulation performance of the metal parts and extending the service life.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116478619B_ABST
    Figure CN116478619B_ABST
Patent Text Reader

Abstract

The present invention provides a method for forming a silicone layer on the surface of a metal part, the method comprising the following steps: batching: prepare material A and material B according to the following components, and then evenly mix material A and material B in a ratio of 1:1 to obtain an AB mixture; take the metal part to be formed with a silicone layer, and clean the surface of the metal part; spray molding: use a spraying device to spray the AB mixture on the surface of the cleaned metal part according to a preset process, so that a silicone layer is formed on the surface of the metal part, and the preset process is repeated for a number of times to reach a preset thickness of the silicone layer. The present invention also provides a silicone layer, which is prepared by mixing material A and material B in a ratio of 1:1. Compared with the related art, the method for forming a silicone layer on the surface of a metal part of the present invention makes the silicone layer more firm, has a good texture, and has high production efficiency after being formed on the surface of the metal part, and the silicone layer itself has high tensile strength and tear strength.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of metal part surface treatment, and in particular to a method for forming a silicone layer on the surface of a metal part and the silicone layer. Background Art

[0002] In our daily life, metal parts can be seen everywhere, such as thermos cups, pots, buckets, etc. Compared with plastic parts, they are stronger and have a longer service life.

[0003] However, metal parts are not heat-insulated, have a monotonous appearance, and are easily oxidized over time, making their appearance unsightly. Therefore, most metal parts are painted on the surface to form a protective layer, and various patterns are formed by spraying paint to improve their service life and appearance. However, the painted metal parts still have the problems of poor texture and lack of heat insulation, resulting in a poor user experience. Therefore, a layer of silicone is wrapped around the metal parts to overcome the problems of poor texture and lack of heat insulation.

[0004] However, in the prior art, the metal parts wrapped in silicone structure adopt a process of one-piece molding using a mold. This production method is inefficient and requires mold coordination, which increases production costs. The metal parts are easily crushed and deformed during one-piece molding, and the tensile strength of the silicone itself is insufficient, so it is easy to fall off after a period of use.

[0005] Therefore, it is necessary to provide a new method for forming a silicone layer on the surface of a metal part and a silicone layer to solve the above problems. Summary of the invention

[0006] The technical problem to be solved by the present invention is to provide a method for forming a silicone layer on the surface of a metal part and a silicone layer, wherein the method makes the silicone layer more firm, has a good texture and high production efficiency after being formed on the surface of the metal part.

[0007] In order to solve the above technical problems, an embodiment of the present invention provides a method for forming a silicone layer on the surface of a metal part, the method comprising the following steps:

[0008] Ingredients: Prepare material A and material B according to the following composition, and then mix the material A and the material B in a ratio of 1:1 to obtain an AB mixture; wherein:

[0009] The material A is composed of the following components by mass percentage:

[0010] Vinyl silicone oil, 30-50%;

[0011] Platinum water, 0.10-0.15%;

[0012] Silane coupling agent, 3-4.9%;

[0013] Fumed silica, 25-30%;

[0014] Aluminum hydroxide, 20-30%;

[0015] The B material is composed of the following components by mass percentage:

[0016] Vinyl silicone oil, 50%;

[0017] inhibitor, 0.10%;

[0018] Silane coupling agent, 4.90%;

[0019] Fumed silica, 25%;

[0020] Aluminum hydroxide, 20%;

[0021] Take the metal part to be molded with the silicone layer and clean the surface of the metal part: degreasing and sanding the surface of the metal part in turn, then cleaning it with alcohol and drying it;

[0022] Spraying molding: using a spraying device to spray the AB mixture on the surface of the cleaned metal part according to a preset process, so that a silicone layer is formed on the surface of the metal part; wherein the preset process includes spraying, baking, and inspection in sequence; the preset process is repeated for a number of times to reach a preset thickness of the silicone layer;

[0023] The spraying process specifically includes:

[0024] Spraying the surface of the metal part at intervals to form a plurality of first spraying areas spaced apart from each other on the surface of the metal part;

[0025] The surface of the metal part is sprayed again at intervals to form a plurality of second spraying areas spaced from each other, so that each of the second spraying areas is located between two adjacent first spraying areas and partially overlaps with the two first spraying areas respectively; the plurality of first spraying areas and the plurality of second spraying areas completely cover the surface of the metal part;

[0026] The surface of the metal part is finally sprayed continuously to form a continuous overall spraying area, and the overall spraying area completely covers the first spraying area and the second spraying area.

[0027] Preferably, in the AB mixture:

[0028] Material A is composed of the following components by mass percentage: 50% vinyl silicone oil, 0.1% platinum water, 4.9% silane coupling agent, 25% fumed silica, and 20% aluminum hydroxide;

[0029] Material B is composed of the following components by mass percentage: 50% vinyl silicone oil, 0.1% inhibitor, 4.9% silane coupling agent, 25% fumed silica, and 20% aluminum hydroxide.

[0030] Preferably, before the spraying step, the following steps are also included:

[0031] According to different needs, the AB mixture is diluted 1-8 times with white starch oil before spraying.

[0032] Preferably, the metal part is a stainless steel cup. Before the spray molding step, the AB mixture is diluted 2-3 times with white starch oil before spraying; in the spray molding step, the preset process is cycled 3-5 times; the inspection process is to inspect the thickness and appearance of the sprayed AB mixture.

[0033] Preferably, the metal is an air fryer fan blade. Before the spraying and molding step, the AB mixture is diluted 3-6 times with white starch oil before spraying; in the spraying and molding step, the preset process is cycled once; the inspection process is to inspect the thickness and appearance of the sprayed AB mixture.

[0034] Preferably, in the preset process, the baking conditions are: baking temperature 225-235° C., baking time 4-6 minutes.

[0035] Preferably, in the preset process, the baking conditions are: baking temperature 230° C., baking time 5 minutes.

[0036] Preferably, the first spraying area, the second spraying area and the overall spraying area are all formed by uniform speed spraying.

[0037] The embodiment of the present invention further provides a silicone layer, which is used to be molded on the surface of a metal part, and is obtained by uniformly mixing material A and material B in a ratio of 1:1; wherein:

[0038] The material A is composed of the following components by mass percentage:

[0039] Vinyl silicone oil, 30-50%;

[0040] Platinum water, 0.10-0.15%;

[0041] Silane coupling agent, 3-4.9%;

[0042] Fumed silica, 25-30%;

[0043] Aluminum hydroxide, 20-30%;

[0044] The B material is composed of the following components by mass percentage:

[0045] Vinyl silicone oil, 50%;

[0046] inhibitor, 0.10%;

[0047] Silane coupling agent, 4.90%;

[0048] Fumed silica, 25%;

[0049] Aluminum hydroxide, 20%.

[0050] Compared with the prior art, the silicone layer of the present invention controls the components and the mass percentage of each component. Platinum water makes the material molecules cross-linked into network structure molecules, the inhibitor can effectively control the cross-linking speed of the material molecules, the silane coupling agent makes the components more effectively mixed together, and the fumed white carbon effectively improves the strength, so that the silicone layer formed on the surface of the metal part not only has good texture, heat insulation and beauty, but also the tensile strength of the formed silicone layer itself is greater than 6MPA, the tear strength is greater than 20N / MM, and it can be boiled in water for 4 hours without falling off, which effectively improves the reliability and service life, and the user experience is better. The molding is achieved through a spraying process, the operation is simple, and the production efficiency is high. BRIEF DESCRIPTION OF THE DRAWINGS

[0051] The present invention will be described in detail below in conjunction with the accompanying drawings. The above and other aspects of the present invention will become clearer and easier to understand through the detailed description made in conjunction with the following drawings. In the accompanying drawings:

[0052] Figure 1 This is a flowchart of a method for forming a silicone layer on a metal surface according to an embodiment of the present invention;

[0053] Figure 2 It is a schematic diagram of the spraying process in the method for forming a silicone layer on a metal surface according to an embodiment of the present invention. DETAILED DESCRIPTION

[0054] The present invention will be further described below in conjunction with the embodiments.

[0055] The specific implementation modes / embodiments recorded herein are specific implementation modes of the present invention, which are used to illustrate the concept of the present invention, are explanatory and exemplary, and should not be interpreted as limiting the implementation modes of the present invention and the scope of the present invention. In addition to the embodiments recorded herein, those skilled in the art can also adopt other obvious technical solutions based on the contents disclosed in the claims and the specification of this application, and these technical solutions include any obvious replacement and modification of the embodiments recorded herein, which are within the protection scope of the present invention.

[0056] Please combine Figure 1 As shown, an embodiment of the present invention provides a method for forming a silicone layer on the surface of a metal part, the method comprising the following steps:

[0057] Step S1, ingredients: prepare material A and material B according to the following composition, and then mix the material A and the material B in a ratio of 1:1 to obtain a mixed material AB.

[0058] The material A is composed of the following components by mass percentage:

[0059] Vinyl silicone oil, 30-50%; platinum water, 0.10-0.15%; silane coupling agent, 3-4.9%; fumed silica, 25-30%; aluminum hydroxide, 20-30%.

[0060] Vinyl silicone oil is the main base material of material A.

[0061] Platinum water is a platinum vulcanizing agent, which is mainly used to cross-link material molecules into a network structure. Because the uncross-linked material is a linear molecular structure with poor strength and other properties, after cross-linking, a network structure is formed, and the strength and other properties are greatly improved, with better strength and other properties, especially tear strength and tensile strength.

[0062] Silane coupling agent is used to make the components mix better. Because material A is in liquid form, the compatibility of the components is different. Adding coupling agent can effectively improve the compatibility of the components and improve the performance of material A.

[0063] Fumed silica is used to improve the strength of A material.

[0064] Aluminum hydroxide is used as a filler and flame retardant.

[0065] The B material is composed of the following components by mass percentage:

[0066] Vinyl silicone oil, 50%;

[0067] inhibitor, 0.10%;

[0068] Silane coupling agent, 4.90%;

[0069] Fumed silica, 25%;

[0070] Aluminum hydroxide, 20%.

[0071] Vinyl silicone oil is used as the main base material of B material.

[0072] The function of the silane coupling agent is the same as that in material A.

[0073] The inhibitor is used to control the cross-linking speed of each component material. If the cross-linking speed of each component material is fast, the B material will mature (form) quickly, and the cross-linking will be completed without spraying, which is difficult to produce. If the cross-linking speed is slow, it will affect the production efficiency and process stability. Therefore, increasing the inhibitor according to the above mass percentage effectively ensures the production efficiency and process stability, and can quickly achieve forming after spraying.

[0074] It should be noted that in this method, material A and material B are first prepared separately, and then material A and material B are mixed to obtain AB mixture before spraying when they are needed. Because the platinum water in material A is a platinum vulcanizing agent, it can react and cross-link with the inhibitor in material B. Material A and material B are easily cross-linked after mixing, which affects the storage time. Therefore, in this method, material A and material B are prepared separately, which effectively increases the storage time.

[0075] Step S2, take the metal piece to be formed with the silicone layer and clean the surface of the metal piece. The surface cleaning of the metal piece includes degreasing or sanding the surface of the metal piece in sequence, then cleaning it with alcohol and drying it.

[0076] In this embodiment, degreasing and sanding have the same purpose, in order to remove oil and impurities on the surface of the metal part to avoid poor adhesion affecting the adhesion effect of the molded silicone layer, and then the purpose of cleaning with alcohol is to ensure the surface is clean and further improve the adhesion.

[0077] Step S3, dilute the AB mixture by 1-8 times with white starch oil according to different needs and then spray. Of course, this step is not necessary, and the AB mixture can also be directly sprayed without dilution.

[0078] In this embodiment, the AB mixture is diluted as needed by using white starch oil before use. White starch oil itself has no significant effect on the performance of the AB mixture, and only plays a diluting role. If the AB mixture is not diluted, it will be too concentrated, the spray flow rate will be very small, the production efficiency will be low, and the molding effect will be poor; and if the formula of the above-mentioned percentage mass ratio components of the present invention is diluted too much, the AB mixture will be too thin, the spraying thickness will be insufficient, and the molding strength will also be affected.

[0079] Step S4, spraying and molding: using a spraying device to spray the AB mixture on the surface of the cleaned metal part according to a preset process, so that a silicone layer is formed on the surface of the metal part.

[0080] The preset steps include spraying, baking and inspection in sequence. According to the requirements of the thickness of the silicone layer of different product moldings, the preset thickness of the silicone layer is achieved by cycling the preset steps for a certain number of times.

[0081] Specific, combined Figure 2 As shown, taking a rectangular metal piece as an example, in the preset process, the spraying process specifically includes:

[0082] Step S41 , spraying the surface of the metal part at intervals to form a plurality of first spraying areas 10 spaced apart from each other on the surface of the metal part.

[0083] Step S42, spraying the surface of the metal part again at intervals to form a plurality of second spraying areas 20 spaced apart from each other, so that each of the second spraying areas 20 is located between two adjacent first spraying areas 10, and partially overlaps with the two first spraying areas 10 respectively; the plurality of first spraying areas 10 and the plurality of second spraying areas 20 completely cover the surface of the metal part.

[0084] In this sub-step, that is, each group of adjacent first spraying areas 10 and second spraying areas 20 have overlapping areas, which is equivalent to dividing an entire surface of the AB mixture layer into multiple small areas for separate attachment, and the multiple small areas are attached to each other in pairs to form a first locking structure, which can effectively decompose the external force into multiple strands and reduce it. This sub-process setting can effectively avoid the phenomenon that when a small part of the entire surface of the AB mixture layer is unstable, the entire surface of the AB mixture layer will become unstable and weak and thus easy to fall off, which effectively improves the reliability tensile strength.

[0085] Step S43, the surface of the metal part is sprayed continuously to form a continuous overall spraying area, and the overall spraying area completely covers the first spraying area 10 and the second spraying area 20. This sub-step forms a second overall lock connection between the first spraying area 10 and the second spraying area 20 to further improve reliability. At the same time, the overall spraying area formed by continuous spraying can also control the thickness of the silicone layer formed by a complete spraying process through the spraying speed. Of course, since each complete spraying process is divided into three sub-spraying processes, the difference in thickness formed is also very small, and can even be ignored.

[0086] More preferably, in this method, the first spraying area 10, the second spraying area 20 and the overall spraying area are all formed by spraying at a uniform speed, which can further improve the control accuracy of the thickness of the final formed silicone layer.

[0087] The division of the first spraying area 10 and the second spraying area 20 can be set as needed. Spraying is achieved by controlling the movement of the spraying equipment or the movement of the metal parts. This is easy to understand and implement. The division method is not limited to one method and will not be described in detail here.

[0088] When spraying, use a special spray gun in the spray workshop, or use an automatic spray line to spray. The spraying area can be separated according to the surface area of ​​different products. The shape of the nozzle and the size of the spraying surface can also be adjusted. These are all easy to think of and easy to achieve.

[0089] The baking conditions are: baking temperature 225-235° C., baking time 4-6 minutes.

[0090] The inspection is to inspect the thickness and appearance structure achieved after each preset process is completed.

[0091] In the method for forming a silicone layer on a metal surface of the present invention, the silicone layer can be boiled in water for 4 hours without falling off after being formed, and can also pass a 100-grid peeling test. The performance of the silicone layer material itself can achieve a tensile strength greater than 6MPA and a tear strength greater than 20N / MM.

[0092] Two specific examples are provided below to further illustrate:

[0093] Embodiment 1

[0094] In this embodiment, the metal piece is taken as a stainless steel cup.

[0095] Step S101, batching: prepare material A and material B according to the following composition, and then mix the material A and the material B in a ratio of 1:1 to obtain an AB mixture.

[0096] Wherein, material A is composed of the following components by mass percentage: 50% vinyl silicone oil, 0.1% platinum water, 4.9% silane coupling agent, 25% fumed silica, and 20% aluminum hydroxide.

[0097] Material B is composed of the following components by mass percentage: 50% vinyl silicone oil, 0.1% inhibitor, 4.9% silane coupling agent, 25% fumed silica, and 20% aluminum hydroxide.

[0098] Step S102, taking a stainless steel cup with a silicone layer to be formed, and cleaning the surface of the stainless steel cup, including degreasing and sanding the surface of the stainless steel cup in sequence, and then cleaning it with alcohol and drying it.

[0099] Step S103, diluting the AB mixture by 2-3 times with white starch oil before spraying.

[0100] Step S104, spraying and forming: spray the AB mixture on the surface of the cleaned stainless steel cup according to the preset process using a spraying device, so that a silicone layer is formed on the surface of the stainless steel cup. The preset process is cycled 3-5 times. In the baking sub-process in each cycle, the baking temperature is 230°C and the baking time is 5 minutes.

[0101] In this embodiment, the silicone layer can be boiled in water for 4 hours without falling off after being formed, and can also pass a 100-grid peeling test. The performance of the silicone layer material itself can achieve a tensile strength greater than 6.5 MPA and a tear strength greater than 22 N / MM.

[0102] Embodiment 2

[0103] In this embodiment, the metal part takes a metal fan blade used in an air fryer as an example.

[0104] Step S201, batching: prepare material A and material B according to the following composition, and then mix the material A and the material B in a ratio of 1:1 to obtain an AB mixture.

[0105] Wherein, material A is composed of the following components by mass percentage: 50% vinyl silicone oil, 0.1% platinum water, 4.9% silane coupling agent, 25% fumed silica, and 20% aluminum hydroxide.

[0106] Material B is composed of the following components by mass percentage: 50% vinyl silicone oil, 0.1% inhibitor, 4.9% silane coupling agent, 25% fumed silica, and 20% aluminum hydroxide.

[0107] Step S202, taking the metal fan blade with the silicone layer to be formed, and cleaning the surface of the metal fan blade, including degreasing and sanding the surface of the metal fan blade in sequence, and then cleaning it with alcohol and drying it.

[0108] Step S203, diluting the AB mixture by 3-6 times with white starch oil before spraying.

[0109] Step S204, spraying molding: Use a spraying device to spray the AB mixture on the surface of the cleaned metal fan blade according to a preset process, so that a silicone layer is formed on the surface of the metal fan blade. The preset process is cycled once. In the baking sub-process in each cycle, the baking temperature is 230°C and the baking time is 5 minutes.

[0110] In this embodiment, the silicone layer can be boiled in water for 4 hours without falling off after being formed, and can also pass a 100-grid peeling test. The performance of the silicone layer material itself can achieve a tensile strength greater than 6.1 MPA and a tear strength greater than 21 N / MM.

[0111] The embodiment of the present invention further provides a silicone layer, which is used to be molded on the surface of a metal part, and is obtained by uniformly mixing material A and material B in a ratio of 1:1; wherein:

[0112] The material A is composed of the following components by mass percentage:

[0113] Vinyl silicone oil, 30-50%; platinum water, 0.10-0.15%; silane coupling agent, 3-4.9%; fumed silica, 25-30%; aluminum hydroxide, 20-30%.

[0114] The B material is composed of the following components by mass percentage:

[0115] Vinyl silicone oil, 50%; inhibitor, 0.10%; silane coupling agent, 4.90%; fumed silica, 25%; aluminum hydroxide, 20%.

[0116] After being formed, the silicone layer of the present invention can be boiled in water for 4 hours without falling off, and can also pass a 100-grid peeling test. The performance of the silicone layer material itself can achieve a tensile strength greater than 6MPA and a tear strength greater than 20N / MM.

[0117] Compared with the prior art, the silicone layer of the present invention controls the components and the mass percentage of each component. Platinum water makes the material molecules cross-linked into network structure molecules, the inhibitor can effectively control the cross-linking speed of the material molecules, the silane coupling agent makes the components more effectively mixed together, and the fumed white carbon effectively improves the strength, so that the silicone layer formed on the surface of the metal part not only has good texture, heat insulation and beauty, but also the tensile strength of the formed silicone layer itself is greater than 6MPA, the tear strength is greater than 20N / MM, and it can be boiled in water for 4 hours without falling off, which effectively improves the reliability and service life, and the user experience is better. The molding is achieved through a spraying process, the operation is simple, and the production efficiency is high.

[0118] The above descriptions are merely embodiments of the present invention and are not intended to limit the patent scope of the present invention. Any equivalent structure or equivalent process transformation made using the contents of the present invention specification and drawings, or directly or indirectly applied in other related technical fields, are also included in the patent protection scope of the present invention.

Claims

1. A method for forming a silicone layer on the surface of a metal part, characterized in that: The method comprises the following steps: Ingredients: Prepare material A and material B according to the following composition, and then mix the material A and the material B in a ratio of 1:1 to obtain an AB mixture; wherein: The material A is composed of the following components by mass percentage: Vinyl silicone oil, 30-50%; Platinum water, 0.10-0.15%; Silane coupling agent, 3-4.9%; Fumed silica, 25-30%; Aluminum hydroxide, 20-30%; The sum of the mass percentages of each component of material A is equal to 100%; The B material is composed of the following components by mass percentage: Vinyl silicone oil, 50%; inhibitor, 0.10%; Silane coupling agent, 4.90%; Fumed silica, 25%; Aluminum hydroxide, 20%; Take the metal part to be molded with the silicone layer and clean the surface of the metal part: degreasing and sanding the surface of the metal part in turn, then cleaning it with alcohol and drying it; Spraying molding: using a spraying device to spray the AB mixture on the surface of the cleaned metal part according to a preset process, so that a silicone layer is formed on the surface of the metal part; wherein the preset process includes spraying, baking, and inspection in sequence; the preset process is repeated for a number of times to reach a preset thickness of the silicone layer; The spraying process specifically includes: Spraying the surface of the metal part at intervals to form a plurality of first spraying areas spaced apart from each other on the surface of the metal part; The surface of the metal part is sprayed again at intervals to form a plurality of second spraying areas spaced from each other, so that each of the second spraying areas is located between two adjacent first spraying areas and partially overlaps with the two first spraying areas respectively; the plurality of first spraying areas and the plurality of second spraying areas completely cover the surface of the metal part; The surface of the metal part is finally sprayed continuously to form a continuous overall spraying area, and the overall spraying area completely covers the first spraying area and the second spraying area.

2. The method for forming a silicone layer on the surface of a metal part according to claim 1, characterized in that: In the AB mixture: Material A is composed of the following components by mass percentage: 50% vinyl silicone oil, 0.1% platinum water, 4.9% silane coupling agent, 25% fumed silica, and 20% aluminum hydroxide; Material B is composed of the following components by mass percentage: 50% vinyl silicone oil, 0.1% inhibitor, 4.9% silane coupling agent, 25% fumed silica, and 20% aluminum hydroxide.

3. The method for forming a silicone layer on the surface of a metal part according to claim 1, characterized in that: Before the spraying step, the method further includes the following steps: According to different needs, the AB mixture is diluted 1-8 times with white starch oil before spraying.

4. The method for forming a silicone layer on the surface of a metal part according to claim 3, characterized in that: The metal part is a stainless steel cup. Before the spraying and molding step, the AB mixture is diluted 2-3 times with white starch oil before spraying; in the spraying and molding step, the preset process is cycled 3-5 times; the inspection process is to inspect the thickness and appearance of the sprayed AB mixture.

5. The method for forming a silicone layer on the surface of a metal part according to claim 3, characterized in that: The metal is an air fryer fan blade. Before the spraying and molding step, the AB mixture is diluted 3-6 times with white starch oil before spraying; in the spraying and molding step, the preset process is cycled once; the inspection process is to inspect the thickness and appearance of the sprayed AB mixture.

6. The method for forming a silicone layer on the surface of a metal part according to claim 1, characterized in that: In the preset process, the baking conditions are: baking temperature 225-235° C., baking time 4-6 minutes.

7. The method for forming a silicone layer on the surface of a metal part according to claim 6, characterized in that: In the preset process, the baking conditions are: baking temperature 230° C., baking time 5 minutes.

8. The method for forming a silicone layer on the surface of a metal part according to claim 7, characterized in that: The first spraying area, the second spraying area and the overall spraying area are all formed by spraying at a uniform speed.