Ceramic substrate with double-sided metal coating and preparation method thereof
By designing honeycomb or grid-shaped semi-etched grooves on the ceramic substrate and adjusting the area and depth of the etched groove, the thermal stress problem of the ceramic copper-clad substrate under hot and cold shock is solved, and the reliability and reliability of the ceramic substrate are significantly improved. life.
Patent Information
- Application Number
- CN202210052397.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-01-18
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2042-01-18
AI Technical Summary
The thermal stress problem of ceramic copper-clad substrates due to the CTE difference between the metal layer and the ceramic under hot and cold shocks leads to ceramic cracking and reduced reliability.
Design honeycomb or grid-shaped semi-etched grooves on the metal layer of the ceramic substrate, and reduce thermal stress by adjusting the area and depth of the etched grooves. Specific methods include the etching groove area accounting for 5%-40% of the metal surface, and the depth It is 40%-70%, and is differentially adjusted according to the front graphic distribution and residual metal rate.
Effectively releases thermal stress, improves the thermal stress distribution of the ceramic substrate, and improves the reliability and life of the ceramic substrate, especially the performance under hot and cold cycle conditions is increased by more than 5 times.
Smart Images

Figure CN116496098B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of ceramic substrate preparation, and in particular relates to a ceramic substrate with metal cladding on both sides and a preparation method thereof. Background Art
[0002] Miniaturized high-voltage and high-power modules are one of the important development directions of semiconductor devices. In the design of semiconductor devices, as the size decreases, the chip power density increases sharply, which puts forward new requirements for the reliability of module heat dissipation packaging. Ceramic copper-clad substrates are the most excellent packaging materials for power modules in the field of power electronics. Due to the high thermal conductivity of ceramic copper-clad substrates, the heat of the chip can be quickly dissipated to the outside world, and they are generally used as the lining of the chip.
[0003] Ceramic copper-clad substrate is a substrate metallized on the ceramic surface. According to the process, it can be divided into DBC (direct bonding copper-clad ceramic substrate), AMB (active metal brazing ceramic substrate), DPC (direct electroplating copper-clad ceramic substrate), DBA (ceramic aluminum-clad substrate), etc. Ceramic copper-clad substrate has good high temperature resistance and electrical properties. It has high thermal conductivity and carries a large current density. It can be used as an important component of semiconductor refrigerators, electronic heaters, high-power power semiconductor modules, and high-voltage and high-power modules.
[0004] The main factor affecting the life of the ceramic copper-clad substrate comes from the delamination failure between the metal layer and the ceramic. Due to the large difference in CTE (coefficient of thermal expansion) between metal layers such as copper or aluminum and ceramics, when subjected to hot and cold shocks, their bonding surfaces are affected by certain stresses, which eventually leads to ceramic cracking and delamination of copper and ceramics, affecting the reliability of the ceramic copper-clad substrate. Summary of the invention
[0005] The present invention is made to solve the above technical problems. According to the pattern distribution on the pattern surface of the ceramic substrate and the residual metal rate (the ratio of the area covered by metal on the pattern surface to the area of the entire board), the thermal stress on the ceramic substrate under hot and cold shock conditions is reduced by designing honeycomb or grid-shaped half-etched grooves.
[0006] In order to achieve the above object, the technical solution adopted by the present invention is as follows:
[0007] The first aspect of the present invention provides a ceramic substrate with double-sided metal cladding, comprising a ceramic sheet and a front metal layer and a back metal layer respectively arranged on the front and back of the ceramic sheet, wherein the front metal layer is etched with an etching groove and a front graphic area, and the back metal layer is etched with a half-etching groove and a back graphic area. The half-etching groove is in a honeycomb or grid shape, the area of the half-etching groove accounts for 5%-40% of the entire metal surface (the sum of the metal surfaces on the front and back sides), the depth is 40%-70% of the metal surface, and the width of the etching groove is 0.4mm-5mm.
[0008] Preferably, in the double-sided metal-clad ceramic substrate provided by the present invention, the thickness of the ceramic sheet is 0.1 mm-1.0 mm, and the thickness of the front metal layer and the back metal layer are both 0.4 mm-1.0 mm. In the present invention, the front metal layer and the back metal layer are copper layers or aluminum layers, and the method of applying them to the ceramic sheet is direct bonding, active brazing or direct electroplating.
[0009] Preferably, in the double-sided metal-clad ceramic substrate provided by the present invention, when the half-etched groove is honeycomb-shaped, the area of the half-etched groove accounts for 5%-30% of the total metal surface area, and the depth is 40%-70% of the metal surface; when the half-etched groove is grid-shaped, the area of the half-etched groove accounts for 10%-40% of the total metal surface area, and the depth is 40%-70% of the metal surface.
[0010] If the half-etched groove area is too small, it cannot effectively release thermal stress. If the half-etched groove area is too large, the incremental effect of releasing thermal stress is extremely small, and it will increase the risk of stress mismatch between the back metal layer and the front metal layer, causing the copper clad laminate to warp. When the depth of the half-etched groove is less than 40%, the effect of releasing thermal stress is poor, but when the depth is too large and exceeds 70%, it will have a significant adverse effect on the heat dissipation performance of the back of the substrate.
[0011] Preferably, in the ceramic substrate with double-sided metal cladding provided by the present invention, the method for determining the area of the half-etched groove is as follows: taking each 1 / 16 of the front graphic surface area as a block, when the difference in residual metal rate between blocks exceeds 10%, the area ratio of the back half-etched groove corresponding to different blocks is adjusted differentially, and the block with a high residual metal rate of the front graphic has a 10%-50% higher back half-etched groove area than the block with a low residual metal rate. Specifically:
[0012] When the residual metal rate of the front pattern is below 40%, if a honeycomb half-etched groove is used, the area of the half-etched groove accounts for 20%-30% of the entire metal surface, the depth is 50%-60% of the metal surface, and the width of the etching groove is 1mm-2mm; if a grid-shaped half-etched groove is used, the area of the half-etched groove accounts for 30%-40% of the entire metal surface, the depth is 60%-70% of the metal surface, and the width of the etching groove is 1mm-5mm;
[0013] When the residual metal rate of the front pattern is 40%-70%, if a honeycomb half-etched groove is used, the area of the half-etched groove accounts for 10%-20% of the entire metal, the depth is 45%-50% of the metal surface, and the width of the etching groove is 1mm-2mm; if a grid-shaped half-etched groove is used, the area of the half-etched groove accounts for 20%-30% of the entire metal surface, the depth is 45%-50% of the metal surface, and the width of the etching groove is 1mm-5mm;
[0014] When the residual metal rate is between 70% and 95%, if a honeycomb half-etched groove is used, the area of the half-etched groove accounts for 5% to 10% of the entire metal surface, the depth is 40% to 45% of the metal surface, and the width of the etching groove is 0.4mm to 1mm; if a grid-shaped half-etched groove is used, the area of the half-etched groove accounts for 20% to 30% of the entire metal surface, the depth is 40% to 45% of the metal surface, and the width of the etching groove is 0.4mm to 1mm.
[0015] A second aspect of the present invention provides a method for preparing a ceramic substrate with metal cladding on both sides, comprising the following steps:
[0016] S1) Ceramic sheet metal bonding: copper or aluminum and ceramic sheet are bonded on both sides by active brazing, direct bonding, or electroplating and chemical plating;
[0017] S2) Surface treatment: Use an organic degreasing agent and a sulfuric acid solution to degrease and micro-etch the surface. The sulfuric acid solution is an aqueous solution containing 2%-4% sulfuric acid and 40-80g / L sodium sulfate;
[0018] S3) Film pasting, exposure, and development: Paste the organic dry film on both sides of the copper-clad board, use a film with a refined spot pattern design for alignment exposure to expose the product pattern on the front side and expose the functional half-etched groove on the back side, and develop after exposure to achieve a one-step method for preparing the half-etched groove;
[0019] S4) Etching of metal layer and solder layer: Copper etching solution is used for metal layer etching, and the metal layer etching time is 10min-60min at a temperature of 20-40°C; if active brazing is used to bond the ceramic sheet to the metal layer, solder etching is required, and the solder etching solution is NaOH alkaline etching solution, and the solder layer etching time is 30min-120min at a temperature of 25°C-50°C.
[0020] Preferably, in step S3), the fine spot design of the film means leaving a spot area on the light-shielding portion of the back of the film without applying the paint; the back of the film is attached to the back of the ceramic substrate, and the shape of the spot area is a triangle, a circle, a rectangle, or a polygon with five or more sides. The width of the light-shielding portion of the film is the width of the half-etched groove on the back, and the size of the spot area is adjusted according to the width.
[0021] More preferably, the spot area is in the shape of a circular hole, the aperture size is 40-200 μm, and the hole spacing is 40-200 μm. Specifically, when the width of the film shielding part is 0.4 mm-1 mm, the corresponding aperture size is 40-100 μm; when the width of the film shielding part is 1 mm-5 mm, the corresponding spot aperture size is 100 um-200 μm.
[0022] The aperture and the correspondence between the aperture and the width of the light-shielding part of the film are the most critical parts of the one-time method for preparing the half-etched groove of the present invention. If the aperture exceeds 200um, the depth of the half-etched groove will exceed 70% after one etching. If the aperture is less than 40um, the etching efficiency of the liquid entering through the spot is too low, and the depth of the half-etched groove cannot reach 40%; if the aperture does not match the width of the light-shielding part of the film, when the half-etched groove is prepared to the specified depth, the metal layer on the front of the ceramic substrate will not be completely etched, or the side etching will be serious, and the quality control requirements of the product cannot be met.
[0023] The beneficial effects of the present invention are as follows:
[0024] In the present invention, preparing a half-etched groove on the back of the ceramic substrate can effectively release thermal stress and improve the thermal stress distribution on the front and back of the ceramic substrate, thereby reducing the failure effect of thermal stress on the ceramic substrate and improving the reliability of the ceramic substrate under hot and cold cycle conditions.
[0025] In terms of preparation, the present invention forms a half-etched groove through a special one-time half-etching process. The size and etching amount of the half-etched groove pattern can be determined according to the front pattern distribution and the residual copper rate. The function of these half-etched grooves is similar to dimple, but the effect is better than dimple. Experiments have shown that the thermal shock performance of 0.32ZTA+0.4 copper thickness is improved by more than 5 times, which improves the reliability of the ceramic substrate under hot and cold cycle conditions, thereby improving the life of the ceramic copper-clad substrate. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 It is a schematic diagram of the structure of a honeycomb half-etched groove;
[0027] Figure 2 It is a schematic diagram of the enlarged structure of the honeycomb half-etched groove;
[0028] Figure 3 It is a schematic diagram of the structure of a grid-shaped half-etched groove;
[0029] Figure 4 The flowchart is for the preparation of a ceramic substrate with metal coating on both sides. DETAILED DESCRIPTION
[0030] The implementation of the present invention is described in detail below in conjunction with the embodiments of the present invention. The following embodiments are implemented on the premise of the technical solution of the present invention, and detailed implementation methods and specific operation processes are given, but the protection scope of the present invention is not limited to the following embodiments.
[0031] 1. Ceramic substrate structure with double-sided metal cladding
[0032] In this embodiment, the ceramic substrate with double-sided metal coating includes a ceramic sheet and a front metal layer and a back metal layer respectively arranged on the front and back of the ceramic sheet. The front metal layer is etched with an etched groove and a front pattern area, and the back metal layer is etched with a half-etched groove and a back pattern area.
[0033] In terms of size, the thickness of the ceramic sheet is 0.1mm-1.0mm, and the thickness of the front metal layer and the back metal layer are both 0.4mm-1.0mm. The front metal layer and the back metal layer are copper layers or aluminum layers, and the method of applying them to the ceramic sheet is direct bonding, active brazing or direct electroplating.
[0034] according to Figure 1 to Figure 3 The shape of the half-etched groove on the back side is honeycomb or grid, and the area of the half-etched groove corresponding to different shapes accounts for different proportions of the entire metal surface area: when the half-etched groove is honeycomb, the area of the half-etched groove accounts for 5%-30% of the entire metal surface area, and the depth is 40%-70% of the metal surface; when the half-etched groove is grid-shaped, the area of the half-etched groove accounts for 10%-40% of the entire metal surface area, and the depth is 40%-70% of the metal surface.
[0035] If the half-etched groove area is too small, it cannot effectively release thermal stress. If the half-etched groove area is too large, the incremental effect of releasing thermal stress is extremely small, and it will increase the risk of stress mismatch between the back metal layer and the front metal layer, causing the copper clad laminate to warp. When the depth of the half-etched groove is less than 40%, the effect of releasing thermal stress is poor, but when the depth is too large and exceeds 70%, it will have a significant adverse effect on the heat dissipation performance of the back of the substrate.
[0036] The method for determining the area of the half-etched groove is as follows: taking every 1 / 16 of the front graphic surface area as a block, when the difference in residual metal rate between blocks exceeds 10%, the proportion of the back half-etched groove area corresponding to different blocks is adjusted differently, and the block with a high residual metal rate of the front graphic has a 10%-50% higher back half-etched groove area than the block with a low residual metal rate.
[0037] Taking copper-clad ceramic substrate as an example, the details are as follows:
[0038] When the residual copper rate of the front pattern is below 40%, if a honeycomb half-etched groove is used, the area of the half-etched groove accounts for 20%-30% of the entire metal surface, the depth is 50%-60% of the metal surface, and the width of the etching groove is 1mm-2mm; if a grid-shaped half-etched groove is used, the area of the half-etched groove accounts for 30%-40% of the entire metal surface, the depth is 60%-70% of the metal surface, and the width of the etching groove is 1mm-5mm;
[0039] When the residual copper rate of the front pattern is 40%-70%, if a honeycomb half-etched groove is used, the area of the half-etched groove accounts for 10%-20% of the entire metal, the depth is 45%-50% of the metal surface, and the width of the etching groove is 1mm-2mm; if a grid-shaped half-etched groove is used, the area of the half-etched groove accounts for 20%-30% of the entire metal surface, the depth is 45%-50% of the metal surface, and the width of the etching groove is 1mm-5mm;
[0040] When the residual copper rate is between 70% and 95%, if a honeycomb half-etched groove is used, the area of the half-etched groove accounts for 5% to 10% of the entire metal surface, the depth is 40% to 45% of the metal surface, and the width of the etching groove is 0.4 mm to 1 mm; if a grid-shaped half-etched groove is used, the area of the half-etched groove accounts for 20% to 30% of the entire metal surface, the depth is 40% to 45% of the metal surface, and the width of the etching groove is 0.4 mm to 1 mm.
[0041] 2. Preparation of ceramic substrate with double-sided metal coating
[0042] See also Figure 4 , including the following steps:
[0043] S1) Ceramic sheet covered with metal
[0044] Active brazing, direct bonding, or electroplating and chemical plating are used to double-side bond copper or aluminum and ceramic sheets.
[0045] S2) Surface treatment
[0046] The surface is degreased, cleaned and micro-etched using an organic degreasing agent and a sulfuric acid solution, wherein the sulfuric acid solution is an aqueous solution containing 2%-4% sulfuric acid and 40-80g / L sodium sulfate.
[0047] S3) Film pasting, exposure and development:
[0048] The organic dry film is double-sidedly attached to the copper-clad board, and a film with a refined spot pattern design is used for registration exposure to expose the product pattern on the front side and the functional half-etched groove on the back side. After exposure, the half-etched groove is prepared by a one-step method, as follows:
[0049] Film fine spot design means leaving a spot area 1 on the black pigmented light-shielding portion of the back of the film without applying pigment; the back of the film is bonded to the back of the ceramic substrate, and the spot area is in the shape of a triangle, circle, rectangle, or a polygon with five or more sides. The width of the film light-shielding portion is the width of the half-etched groove on the back, and the size of the spot area is adjusted according to this width.
[0050] The shape of the spot area 1 is preferably a circular hole, with an aperture size of 40-200 μm and a hole spacing of 40-200 μm. Specifically, when the width of the film shielding part is 0.4 mm-1 mm, the corresponding aperture size is 40-100 μm; when the width of the film shielding part is 1 mm-5 mm, the corresponding spot aperture size is 100 um-200 μm.
[0051] The aperture and the correspondence between the aperture and the width of the light-shielding part of the film are the most critical parts of the one-time method for preparing the half-etched groove of the present invention. If the aperture exceeds 200um, the depth of the half-etched groove will exceed 70% after one etching. If the aperture is less than 40um, the etching efficiency of the liquid entering through the spot is too low, and the depth of the half-etched groove cannot reach 40%; if the aperture does not match the width of the light-shielding part of the film, when the half-etched groove is prepared to the specified depth, the metal layer on the front of the ceramic substrate will not be completely etched, or the side etching will be serious, and the quality control requirements of the product cannot be met.
[0052] S4) Etching of metal layer and solder layer
[0053] Copper etching liquid is used for metal layer etching, and the metal layer etching time is 10min-60min at a temperature of 20-40°C. If active brazing is used to bond the ceramic sheet to the metal layer, solder etching is required. The solder etching liquid is NaOH alkaline etching liquid, and the solder layer etching time is 30min-120min at a temperature of 25°C-50°C.
[0054] The preferred embodiments of the present invention have been specifically described above, but the present invention is not limited to the embodiments. Those skilled in the art may make various equivalent modifications or substitutions without violating the spirit of the present invention. These equivalent modifications or substitutions are all included in the scope defined by the claims of this application.
Claims
1. A ceramic substrate with metal cladding on both sides, characterized in that: The invention comprises a ceramic sheet and a front metal layer and a back metal layer respectively arranged on the front and back of the ceramic sheet, wherein the front metal layer is etched with an etching groove and a front pattern area, and the back metal layer is etched with a half-etching groove and a back pattern area. The half-etched groove is in a honeycomb or grid shape; when the half-etched groove is in a honeycomb shape, the area of the half-etched groove accounts for 5%-30% of the entire metal surface area, and the depth is 40%-70% of the metal surface; when the half-etched groove is in a grid shape, the area of the half-etched groove accounts for 10%-40% of the entire metal surface area, and the depth is 40%-70% of the metal surface. The method for determining the area of the half-etched groove is as follows: taking each 1 / 16 of the area of the front pattern as a block, when the difference in residual metal rate between blocks exceeds 10%, the area ratio of the back half-etched groove corresponding to different blocks is adjusted differentially, and the block with high residual metal rate of the front pattern has a 10%-50% higher area of the back half-etched groove than the block with low residual metal rate, as follows: When the residual metal rate of the front pattern is below 40%, if a honeycomb half-etched groove is used, the area of the half-etched groove accounts for 20%-30% of the entire metal surface, the depth is 50%-60% of the metal surface, and the width of the etching groove is 1mm-2mm; if a grid-shaped half-etched groove is used, the area of the half-etched groove accounts for 30%-40% of the entire metal surface, the depth is 60%-70% of the metal surface, and the width of the etching groove is 1mm-5mm; When the residual metal rate of the front pattern is 40%-70%, if a honeycomb half-etched groove is used, the area of the half-etched groove accounts for 10%-20% of the entire metal, the depth is 45%-50% of the metal surface, and the width of the etching groove is 1mm-2mm; if a grid-shaped half-etched groove is used, the area of the half-etched groove accounts for 20%-30% of the entire metal surface, the depth is 45%-50% of the metal surface, and the width of the etching groove is 1mm-5mm; When the residual metal rate is between 70% and 95%, if a honeycomb half-etched groove is used, the area of the half-etched groove accounts for 5% to 10% of the entire metal surface, the depth is 40% to 45% of the metal surface, and the width of the etching groove is 0.4mm to 1mm; if a grid-shaped half-etched groove is used, the area of the half-etched groove accounts for 20% to 30% of the entire metal surface, the depth is 40% to 45% of the metal surface, and the width of the etching groove is 0.4mm to 1mm. The method for preparing the double-sided metal-clad ceramic substrate is characterized by comprising the following steps: S1) Ceramic sheet metal bonding: copper or aluminum and ceramic sheet are bonded on both sides by active brazing, direct bonding, or electroplating and chemical plating; S2) Surface treatment: Use organic degreasing agent and sulfuric acid solution to degrease and micro-etch the surface; S3) Film pasting, exposure, and development: Paste the organic dry film on both sides of the copper-clad board, use a film with a refined spot pattern design for alignment exposure to expose the product pattern on the front side and the functional half-etched groove on the back side, and develop after exposure; The film fine spot design refers to leaving a spot area on the black pigmented shading portion of the back of the film without applying pigment; the back of the film is bonded to the back of the ceramic substrate, the spot area is in the shape of a triangle, circle, rectangle or a polygon with five or more sides, the width of the film shading portion is the width of the back half-etched groove, and the size of the spot area is adjusted according to the width. The spot area is in the shape of a circular hole, with an aperture size of 40-200μm and a hole spacing of 40-200μm. When the width of the film shading part is 0.4mm-1mm, the corresponding aperture size is 40-100μm; when the width of the film shading part is 1mm-5mm, the corresponding spot aperture size is 100um-200μm. S4) Etching of metal layer and solder layer.
2. The double-sided metal-clad ceramic substrate according to claim 1, characterized in that: in, The thickness of the ceramic sheet is 0.1mm-1.0mm, and the thickness of the front metal layer and the back metal layer are both 0.4mm-1.0mm.
3. The double-sided metal-clad ceramic substrate according to claim 1, characterized in that: in, The front metal layer and the back metal layer are copper layers or aluminum layers, and are applied to the ceramic sheet by direct bonding, active brazing or direct electroplating.
4. The double-sided metal-clad ceramic substrate according to claim 1, Features: Wherein, in step S2), the sulfuric acid solution is an aqueous solution containing 2%-4% sulfuric acid and 40-80g / L sodium sulfate; In step S4), the metal layer is etched with copper etching solution, the metal layer etching time is 10min-60min, and the temperature is 20-40°C; If active brazing is used to bond the ceramic sheet to the metal layer, solder etching is required. The solder etching solution is NaOH alkaline etching solution. The solder layer etching time is 30min-120min and the temperature is 25℃-50℃.